DuPont Performance Polymers Zytel® ST801 NC010A Nylon 66  (Unverified Data**)

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Impact Grade
Manufacturer DuPont Performance Polymers
Trade Name Zytel®
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF DuPont Performance Polymers Zytel® ST801 NC010A Nylon 66  (Unverified Data**).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Super Toughened Polyamide 6 Zytel ST801 is an unreinforced super tough polyamide 66 for injection molding and extrusion. It offers outstanding break resistance over a wide temperature and humidity range and high productivity.Information provided by DuPont Performance Polymers
Physical Properties Metric English Comments
Density 1.08 g/cc
0.0390 lb/in³
DAM; ISO 1183
Water Absorption 6.7 %
<br>@Thickness 2.00 mm
6.7 %
<br>@Thickness 0.0787 in
DAM; Sim. to ISO 62
Moisture Absorption 2.20 %
<br>@Thickness 2.00 mm
2.20 %
<br>@Thickness 0.0787 in
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.017 cm/cm
0.017 in/in
DAM; ISO 294-4 2577
Mechanical Properties Metric English Comments
Tensile Strength, Yield 43.0 MPa
6240 psi
50%RH; ISO 527-1/-2
50.0 MPa
7250 psi
DAM; ISO 527-1/-2
Elongation at Break 32 %
32 %
DAM; Nominal; ISO 527-1/-2
>= 50 %
>= 50 %
50%RH; Nominal; ISO 527-1/-2
Elongation at Yield 5.7 %
5.7 %
DAM; ISO 527-1/-2
37 %
37 %
50%RH; ISO 527-1/-2
Tensile Modulus 0.900 GPa
131 ksi
50%RH; ISO 527-1/-2
2.00 GPa
290 ksi
DAM; ISO 527-1/-2
Shear Modulus 0.0822 GPa
<br>@Temperature 150 °C
11.9 ksi
<br>@Temperature 302 °F
DAM; Dynamic; ISO 11403-1 -2
0.1075 GPa
<br>@Temperature 110 °C
15.59 ksi
<br>@Temperature 230 °F
DAM; Dynamic; ISO 11403-1 -2
0.2994 GPa
<br>@Temperature 60.0 °C
43.42 ksi
<br>@Temperature 140 °F
DAM; Dynamic; ISO 11403-1 -2
0.6815 GPa
<br>@Temperature 10.0 °C
98.84 ksi
<br>@Temperature 50.0 °F
DAM; Dynamic; ISO 11403-1 -2
0.7189 GPa
<br>@Temperature -20.0 °C
104.3 ksi
<br>@Temperature -4.00 °F
DAM; Dynamic; ISO 11403-1 -2
0.9346 GPa
<br>@Temperature -50.0 °C
135.6 ksi
<br>@Temperature -58.0 °F
DAM; Dynamic; ISO 11403-1 -2
Charpy Impact Unnotched NB
NB
DAM; ISO 179/1eU
NB
NB
50%RH; ISO 179/1eU
NB
<br>@Temperature -30.0 °C
NB
<br>@Temperature -22.0 °F
DAM; ISO 179/1eU
NB
<br>@Temperature -30.0 °C
NB
<br>@Temperature -22.0 °F
50%RH; ISO 179/1eU
Charpy Impact, Notched 8.00 J/cm²
38.1 ft-lb/in²
DAM; ISO 179/1eA
11.5 J/cm²
54.7 ft-lb/in²
50%RH; ISO 179/1eA
1.70 J/cm²
<br>@Temperature -30.0 °C
8.09 ft-lb/in²
<br>@Temperature -22.0 °F
50%RH; ISO 179/1eA
1.80 J/cm²
<br>@Temperature -30.0 °C
8.57 ft-lb/in²
<br>@Temperature -22.0 °F
DAM; ISO 179/1eA
Tensile Creep Modulus, 1 hour 1200 MPa
<br>@Time 3600 sec
174000 psi
<br>@Time 1.00 hour
50%RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 750 MPa
<br>@Time 3.60e+6 sec
109000 psi
<br>@Time 1000 hour
50%RH; ISO 899-1
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 120 µm/m-°C
66.7 µin/in-°F
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C
50.0 µin/in-°F
DAM; ISO 11359-1/-2
Melting Point 263 °C
505 °F
DAM; 10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 132 °C
270 °F
DAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 64.0 °C
147 °F
DAM; ISO 75-1/-2
Glass Transition Temp, Tg 75.0 °C
167 °F
DAM; 10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
<br>@Thickness 1.50 mm
HB
<br>@Thickness 0.0591 in
DAM; IEC 60695-11-10
HB
<br>@Thickness 0.800 mm
HB
<br>@Thickness 0.0315 in
DAM; IEC 60695-11-10
Flame Spread 26 mm/min
<br>@Thickness 1.00 mm
1.0 in/min
<br>@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 20 %
20 %
DAM; ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+13 ohm-cm
1.00e+13 ohm-cm
50%RH; IEC 60093
1.00e+15 ohm-cm
1.00e+15 ohm-cm
DAM; IEC 60093
Surface Resistance >= 1.00e+15 ohm
>= 1.00e+15 ohm
50%RH; IEC 60093
Dielectric Constant 2.9
<br>@Frequency 1.00e+6 Hz
2.9
<br>@Frequency 1.00e+6 Hz
DAM; IEC 60250
3.2
<br>@Frequency 100 Hz
3.2
<br>@Frequency 100 Hz
DAM; IEC 60250
3.6
<br>@Frequency 1.00e+6 Hz
3.6
<br>@Frequency 1.00e+6 Hz
50%RH; IEC 60250
8.0
<br>@Frequency 100 Hz
8.0
<br>@Frequency 100 Hz
50%RH; IEC 60250
Dielectric Strength 31.0 kV/mm
787 kV/in
DAM; IEC 60243-1
39.0 kV/mm
991 kV/in
50%RH; IEC 60243-1
Dissipation Factor 0.0080
<br>@Frequency 100 Hz
0.0080
<br>@Frequency 100 Hz
DAM; IEC 60250
0.014
<br>@Frequency 1.00e+6 Hz
0.014
<br>@Frequency 1.00e+6 Hz
DAM; IEC 60250
0.055
<br>@Frequency 1.00e+6 Hz
0.055
<br>@Frequency 1.00e+6 Hz
50%RH; IEC 60250
0.18
<br>@Frequency 100 Hz
0.18
<br>@Frequency 100 Hz
50%RH; IEC 60250
Comparative Tracking Index 600 V
600 V
DAM; IEC 60112
Descriptive Properties Value Comments
Emission of organic compounds 38.4 µgC/g
VDA 277
Odour class 3
VDA 270
Part Marking Code >PA66-HI<
ISO 11469
Processing Injection Moulding
Other Extrusion
Regional Availability Europe
Near East/Africa
Resin Identification PA66-HI