Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 1.40 g/cc @Temperature 23.0 °C |
0.0506 lb/in³ @Temperature 73.4 °F |
ISO 1183 |
Filler Content | 35 % | 35 % | ISO 1172 |
Water Absorption | 1.8 - 2.0 % @Temperature 70.0 °C |
1.8 - 2.0 % @Temperature 158 °F |
62% r.h., Humidity; ISO 62 |
Water Absorption at Saturation | 4.7 - 5.3 % @Time 82800 sec |
4.7 - 5.3 % @Time 23.0 hour |
ISO 62 |
Linear Mold Shrinkage, Flow | 0.0020 cm/cm | 0.0020 in/in | ISO 294-4 |
Linear Mold Shrinkage, Transverse | 0.013 cm/cm | 0.013 in/in | ISO 294-4 |
Spiral Flow | 77.0 cm | 30.3 in | Cross Section: 7[mm]x3.5[mm]; AKRO |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Ball Indentation Hardness | 255 MPa | 37000 psi | H 961/3000; ISO 2039-1 |
Tensile Strength at Break | 215 MPa | 31200 psi | 5 [mm/min]; ISO 527-1/2 |
107.5 MPa @Temperature 160 - 175 °C, Time 1.80e+7 sec |
15590 psi @Temperature 320 - 347 °F, Time 5000 hour |
5 [mm/min], 50% Loss of Tensile Strength; ICE 216 | |
107.5 MPa @Temperature 130 - 150 °C, Time 7.20e+7 sec |
15590 psi @Temperature 266 - 302 °F, Time 20000 hour |
5 [mm/min], 50% Loss of Tensile Strength; ICE 216 | |
Elongation at Break | 3.0 % | 3.0 % | 5 [mm/min]; ISO 527-1/2 |
Tensile Modulus | 11.6 GPa | 1680 ksi | 1[mm/min]; ISO 527-1/2 |
Flexural Strength | 300 MPa | 43500 psi | 2 [mm/min]; ISO 178 |
Flexural Modulus | 10.0 GPa | 1450 ksi | 2 [mm/min]; ISO 178 |
Charpy Impact Unnotched | 9.00 J/cm² @Temperature -30.0 °C |
42.8 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eU |
9.20 J/cm² @Temperature 23.0 °C |
43.8 ft-lb/in² @Temperature 73.4 °F |
ISO 179/1eU | |
Charpy Impact, Notched | 1.30 J/cm² @Temperature -30.0 °C |
6.19 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eA |
1.50 J/cm² @Temperature 23.0 °C |
7.14 ft-lb/in² @Temperature 73.4 °F |
ISO 179/1eA |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
Melting Point | 262 °C | 504 °F | ISO 11357-1/3 |
Deflection Temperature at 0.46 MPa (66 psi) | 260 °C | 500 °F | HDT/B; ISO 75-2 |
Deflection Temperature at 1.8 MPa (264 psi) | 255 °C | 491 °F | HDT/A; ISO 75-2 |
Deflection Temperature at 8.0 MPa | 220 °C | 428 °F | HDT/C; ISO 75-2 |
Flammability, UL94 | HB @Thickness 1.60 mm |
HB @Thickness 0.0630 in |
|
Glow Wire Test | 650 °C @Thickness 1.60 mm |
1200 °F @Thickness 0.0630 in |
ICE 60695-12 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 1.00e+13 ohm-cm | 1.00e+13 ohm-cm | IEC 60093 |
Surface Resistance | 1.00e+12 ohm | 1.00e+12 ohm | IEC 60093 |
Comparative Tracking Index | 600 V | 600 V | Test Solution A; IEC 60112 |
Processing Properties | Metric | English | Comments |
---|---|---|---|
Feed Temperature | 60.0 - 80.0 °C | 140 - 176 °F | |
Nozzle Temperature | 280 - 295 °C | 536 - 563 °F | |
Zone 1 | 260 - 300 °C | 500 - 572 °F | |
Zone 2 | 260 - 300 °C | 500 - 572 °F | |
Zone 3 | 260 - 300 °C | 500 - 572 °F | |
Zone 4 | 260 - 300 °C | 500 - 572 °F | |
Melt Temperature | 280 - 320 °C | 536 - 608 °F | |
Mold Temperature | 80.0 - 100 °C | 176 - 212 °F | |
Drying Temperature | 80.0 °C | 176 °F | |
Dry Time | 2.00 hour | 2.00 hour | |
Hold Pressure | 30.0 - 80.0 MPa | 4350 - 11600 psi | |
Back Pressure | 5.00 - 10.0 MPa | 725 - 1450 psi |
Descriptive Properties | Value | Comments |
---|---|---|
Rate acc. FMVSS 302 ( | Passed | |
Rate acc. FMVSS 302,( | FMVSS 302, >1 [mm] Thickness | |
Resistance to Oleic acid | Pass | 100% Conc. at 23°C |
Resistance to Acetaldehyde | Fail | 40% Conc. at 23°C |
Resistance to Acetic Acid | Pass | 20% Conc. at 23°C |
Resistance to Acetone | Pass | 100% Conc. at 23°C |
Resistance to Acetonitrile | Pass | 100% Conc. at 23°C |
Resistance to Acrylonitrile | Pass | 100% Conc. at 23°C |
Resistance to Allyl alcohol | Fail | 96% Conc. at 23°C |
Resistance to Amyl alcohol | Pass | 100% Conc. at 23°C |
Resistance to Aqueous Ammonia | Pass | 10% Conc. at 23°C |
Resistance to Benzene | Fail | 100% Conc. at 40°C |
Pass | 100% Conc. at 23°C | |
Pass | 100% Conc. at 23°C | |
Resistance to Biodiesel | Pass | 100% Conc. at 23°C |
Resistance to Boric acid | Fail | 100% Conc. at 23°C |
Pass | 10% Conc. at 23°C | |
Resistance to Brake fluid (DOT 4) | Fail | 100% Conc. at 130°C |
Pass | 100% Conc. at 23°C | |
Resistance to Calcium chloride, alcoholic | Fail | 10% Conc. at 23°C |
Resistance to Calcium chloride, aqueous | Pass | 10% Conc. at 23°C |
Resistance to Carbonic acid | Pass | 100% Conc. at 60°C |
Resistance to Caustic potash solution, aqueous | Pass | 50% Conc. at 23°C |
Resistance to Chloracetic acid | Fail | 50% Conc. at 23°C |
Resistance to Chlorine | Fail | 100% Conc. at 23°C |
Resistance to Chlorine water | Fail | 100% Conc. at 23°C |
Resistance to Chromic acid | Fail | 10% Conc. at 23°C |
Resistance to Cyclohexane | Pass | 100% Conc. at 23°C |
Resistance to Cyclohexanol | Pass | 100% Conc. at 23°C |
Resistance to Dichloro-Acetic acid | Fail | 50% Conc. at 23°C |
Resistance to Diesel fuel (DIN 51601) | Pass | 100% Conc. at 23°C |
Resistance to Ethanol | Pass | 96% Conc. at 23°C |
Resistance to Ethylene glycol/water | Fail | 50% Conc. at 120°C |
Resistance to Formaldehyde, aqueous | Pass | 10% Conc. at 23°C |
Resistance to Formic acid | Fail | 2% Conc. at 23°C |
Resistance to Glycerin | Pass | 100% Conc. at 23°C |
Resistance to Hydraulic oil H and HL (DIN 51524) | Pass | 100% Conc. at 100°C |
Resistance to Hydrogen chloride, gas | Fail | 100% Conc. at 23°C |
Resistance to Iso-octanol | Pass | 100% Conc. at 23°C |
Resistance to Isopropanol | Pass | 100% Conc. at 23°C |
Resistance to Methanol | Pass | 100% Conc. at 23°C |
Resistance to Methylene chloride | Fail | 100% Conc. at 23°C |
Resistance to Motor oil (SAE 10W-40) | Pass | 100% Conc. at 130°C |
Pass | 100% Conc. at 23°C | |
Resistance to Natural Gas | Pass | 100% Conc. at 23°C |
Resistance to Nitric acid | Fail | 40% Conc. at 23°C |
Resistance to Ozone | Fail | 100% Conc. at 23°C |
Resistance to Phenol | Fail | 100% Conc. at 23°C |
Resistance to Phosphoric acid | Fail | 30% Conc. at 23°C |
Resistance to Potassium chloride, aqueous | Pass | 10% Conc. at 23°C |
Resistance to Potassium permanganate, aqueous | Fail | 10% Conc. at 23°C |
Resistance to Sodium chloride, aqueous | Pass | 10% Conc. at 23°C |
Resistance to Sodium hydroxide solution, aqueous | Pass | 1% Conc. at 23°C |
Resistance to Sodium hypochlorite, aqueous | Fail | 10% Conc. at 23°C |
Resistance to Transmission oil (ATF m 1375.4) | Pass | 100% Conc. at 150°C |
Resistance to Urea, aqueous | Pass | 20% Conc. at 23°C |
Resistant to Carbon disulphide | Pass | 100% Conc. at 23°C |
Resistant to Carbon tetrachloride | Pass | 100% Conc. at 23°C |
Resistant to Citric acid | Pass | 10% Conc. at 23°C |
Resistant to Ethyl acetate | Pass | 100% Conc. at 23°C |
Resistant to Hydrochloric acid | Fail | 36% Conc. at 23°C |
Resistant to Hydrogen peroxide | Fail | 23°C |
Resistant to Seawater | Pass | 100% Conc. at 23°C |
Resistant to Silicone fluid | Pass | 23°C |
Resistant to Sodium hypochlorite, aqueous | Fail | 5% Conc. at 23°C |
Resistant to Sulphuric acid | Fail | 10% Conc. at 23°C |
Fail | 96% Conc. at 23°C | |
Resistant to Super-grade petrol (DIN 51600) | Pass | 100% Conc. at 23°C |
Resistant to Toluol | Pass | 100% Conc. at 23°C |
Resistant to Water | Pass | 100% Conc. up to 50°C |
Resistant to Xylol | Pass | 100% Conc. at 23°C |
Resistant to Zinc chloride, aqueous | Fail | 50% Conc. at 23°C |