Resinoid 1382 Phenolic Molding, Glass Reinforced

Category Polymer , Thermoset , Filled/Reinforced Thermoset , Phenolic , Phenolic, Novolac, Glass Filled
Manufacturer Resinoid
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Resinoid 1382 Phenolic Molding, Glass Reinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Data provided by the manufacturer.The Resinoid 1300 and 7000 glass fiber reinforced series compounds feature mechanical strength, dimensional stability, electrical insulation, and heat resistance
Physical Properties Metric English Comments
Density 1.89 g/cc
0.0683 lb/in³
ASTM D792A
Linear Mold Shrinkage 0.0010 cm/cm
0.0010 in/in
Positive Mold; ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell E 94
94
ASTM D785
Hardness, Rockwell M 109
109
ASTM D785
Tensile Strength, Ultimate 79.0 MPa
11500 psi
ASTM D651
Flexural Strength 114 MPa
16500 psi
ASTM D790
Flexural Modulus 17.0 GPa
2470 ksi
ASTM D790
Compressive Strength 204 MPa
29600 psi
ASTM D695
Izod Impact, Notched 1.156 J/cm
2.166 ft-lb/in
ASTM D256A
Thermal Properties Metric English Comments
Deflection Temperature at 1.8 MPa (264 psi) >= 315 °C
>= 599 °F
ASTM D648
Electrical Properties Metric English Comments
Dielectric Strength 12.7 kV/mm
323 kV/in
Short Time; Dry; ASTM D149
Arc Resistance 180 sec
180 sec
ASTM D495
Processing Properties Metric English Comments
Mold Temperature 155 - 180 °C
311 - 356 °F