Material Notes:
CORSAIR (M3-1) contains carbon and vanadium levels that are intermediate between those of Double Six (M2) and Crusader (M3-2). This gives the steel a fine balance of wear resistance and grindability. Corsair is an excellent steel for cutting tools such as broaches and form tools where both improved tool life and grindability are important considerations. Typical applications for Corsair high speed steel include form tools, spade drills, milling cutters and broaches.Information Provided by Timken Latrobe Steel.Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.
Physical Properties Metric English Comments
Specific Gravity 8.17 g/cc
8.17 g/cc
Density 8.17 g/cc
0.295 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell C 65
65
Oil Quenched from 1232°C
66.5
66.5
Oil Quenched from 1149°C
66.5
66.5
Oil Quenched from 1177°C
Modulus of Elasticity 207 GPa
30000 ksi
Machinability 40 - 45 %
40 - 45 %
1% Carbon Steel
Izod Impact Unnotched 28.5 J
21.0 ft-lb
Oil Quenched at 1204°C; 510°C Temper Temperature
35.3 J
26.0 ft-lb
Oil Quenched at 1204°C; 482°C Temper Temperature
43.4 J
32.0 ft-lb
Oil Quenched at 1177°C; 482°C Temper Temperature
58.3 J
43.0 ft-lb
Oil Quenched at 1204°C; 622°C Temper Temperature
61.0 J
45.0 ft-lb
Oil Quenched at 1177°C; 622°C Temper Temperature
63.7 J
47.0 ft-lb
Oil Quenched at 1177°C; 566°C Temper Temperature
Thermal Properties Metric English Comments
CTE, linear 11.12 µm/m-°C

@Temperature 21.0 - 204 °C
6.178 µin/in-°F

@Temperature 69.8 - 399 °F
12.4 µm/m-°C

@Temperature 21.0 - 358 °C
6.89 µin/in-°F

@Temperature 69.8 - 676 °F
Component Elements Properties Metric English Comments
Carbon, C 1.02 %
1.02 %
Chromium, Cr 4.1 %
4.1 %
Iron, Fe 80.93 %
80.93 %
Manganese, Mn 0.25 %
0.25 %
Molybdenum, Mo 5.0 %
5.0 %
Silicon, Si 0.30 %
0.30 %
Tungsten, W 6.0 %
6.0 %
Vanadium, V 2.4 %
2.4 %
Chemical Properties Metric English Comments
Critical Temperature 835 °C
1540 °F
Ac1