Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 0.990 g/cc | 0.0358 lb/in³ | ASTM D792 |
Melt Flow | 3.6 g/10 min @Load 2.16 kg, Temperature 235 °C |
3.6 g/10 min @Load 4.76 lb, Temperature 455 °F |
ASTM D1238R |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Hardness, Shore D | 67 | 67 | ASTM D2240 |
Tensile Strength at Break | >= 40.0 MPa | >= 5800 psi | ASTM D638 |
Tensile Strength, Yield | 20.0 MPa | 2900 psi | ASTM D638 |
Elongation at Break | >= 300 % | >= 300 % | ASTM D638 |
Flexural Strength | 16.0 MPa | 2320 psi | ASTM D790 |
Flexural Modulus | 0.330 GPa | 47.9 ksi | ASTM D790 |
Izod Impact, Notched | 6.00 J/cm | 11.2 ft-lb/in | ASTM D256 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
Melting Point | 173 °C | 343 °F | ASTM D3418 |
Deflection Temperature at 0.46 MPa (66 psi) | 126 °C | 259 °F | ASTM D648 |
Processing Properties | Metric | English | Comments |
---|---|---|---|
Processing Temperature | 230 °C | 446 °F | Flange Temperature for T-Die Cast Film Extrusion |
Feed Temperature | 40.0 °C | 104 °F | Injection Molding |
Zone 1 | 190 °C | 374 °F | For T-Die Cast Film Extrusion |
230 °C | 446 °F | For 8x1 mm Tube Extrusion | |
Zone 2 | 210 °C | 410 °F | For T-Die Cast Film Extrusion |
225 °C | 437 °F | For 8x1 mm Tube Extrusion | |
Zone 3 | 220 °C | 428 °F | For 8x1 mm Tube Extrusion |
230 °C | 446 °F | For T-Die Cast Film Extrusion | |
Zone 4 | 215 °C | 419 °F | For 8x1 mm Tube Extrusion |
Die Temperature | 230 °C | 446 °F | For T-Die Cast Film Extrusion |
Mold Temperature | 40.0 - 60.0 °C | 104 - 140 °F | Injection Molding |
Injection Velocity | 100 mm/sec | 3.94 in/sec | Injection Molding |
Die Opening | 0.0400 cm | 0.0157 in | For T-Die Cast Film Extrusion |
Roll Temperature | 50.0 °C | 122 °F | Chill Roll Temperature for T-Die Cast Film Extrusion |
Drying Temperature | 80.0 °C | 176 °F | Option 1 |
100 °C | 212 °F | Option 2 | |
110 °C | 230 °F | Option 3 | |
Dry Time | 2 - 4 hour | 2 - 4 hour | Option 3 |
4 - 6 hour | 4 - 6 hour | Option 2 | |
6 - 8 hour | 6 - 8 hour | Option 1 | |
Injection Pressure | 40.0 - 50.0 MPa | 5800 - 7250 psi | Injection Molding (Injection pressure should be increased when molding thin wall parts. Pressure up to 75 bar can be used here.) |
Hold Pressure | 25.0 - 50.0 MPa | 3630 - 7250 psi | Injection Molding |
Back Pressure | 5.00 MPa | 725 psi | Injection Molding |
Screw Speed | 15 - 76 rpm | 15 - 76 rpm | For 8x1 mm Tube Extrusion |
Descriptive Properties | Value | Comments |
---|---|---|
C/R | 3-3.5:1 | For 8x1 mm Tube Extrusion |
Calibrating Vacuum | 100 mbar | For 8x1 mm Tube Extrusion |
Calibration | 9.95 mm | For 8x1 mm Tube Extrusion |
Compression Ratio | 2.5-3.5:1 | Injection Molding |
min 3:1 | For 8x1 mm Tube Extrusion | |
Die Diameter | 16 mm | For 8x1 mm Tube Extrusion |
Die Width | 300 mm | For T-Die Cast Film Extrusion |
Extractables | 14% | Tolerance (DIN 73378 EtOH 18hr) 2% |
Extruder | Barmag, Screw Diameter = 30 mm | For T-Die Cast Film Extrusion |
Extruder Characteristics | 65 mm screw diameter | For 8x1 mm Tube Extrusion |
Film Thickness | 60 microns | For T-Die Cast Film Extrusion |
Flight Depth in the Feeding Zone | 10-15% of Screw Diameter | Injection Molding |
Flight Depth in the Metering Zone | 5-7% of Screw Diameter | Injection Molding |
Haul Off Speed | 5 m/min | For T-Die Cast Film Extrusion |
Haul Speed | 10-55 m/min | For 8x1 mm Tube Extrusion |
L/D Ratio | 25:1 | For 8x1 mm Tube Extrusion |
min 20:1 | Injection Molding | |
Length of Compression Zone | 25-45% of total screw length | Injection Molding |
30% of screw length | For 8x1 mm Tube Extrusion | |
Length of Feeding Zone | 20-40% of total screw length | Injection Molding |
30-40% of screw length | For 8x1 mm Tube Extrusion | |
Length of Metering Zone | 30-45% of screw length | For 8x1 mm Tube Extrusion |
35-45% of total screw length | Injection Molding | |
Mandrel Diameter | 12 mm | For 8x1 mm Tube Extrusion |
Peripheral screw speed | 10 m/min | Injection Molding |
Water Temperature | 10-18°C | For 8x1 mm Tube Extrusion |