Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Styron Magnum™ AG700 ABS, Low Gloss

Category Polymer , Thermoplastic , ABS Polymer , Acrylonitrile Butadiene Styrene (ABS), Molded
Manufacturer Styron
Trade Name Magnum™
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Styron Magnum™ AG700 ABS, Low Gloss.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ABS resin are available in a wide range of melt flow rates, impact strength and heat resistance for both high and low gloss applications manufactured by injection molding, sheet or profile extrusion and thermoforming.The sheet and thermoforming grades of MAGNUM ABS resins provide excellent high and low gloss aesthetics, good thermal color stability, heat and impact resistance and stiffness for uses such as luggage, tool cases, burial vault liners, signs and recreation vehicle applications. Offering ranges in melt flow rates from 1.0 to 4.0, sheet Izod impacts from 130 to 560 J/m and sheet flexural modulus from 1960 to 2070 MPa, MAGNUM ABS resins can fill a variety of needs.MAGNUM AG700 ABS resin is the lowest gloss and highest melt flow rate option of the MAGNUM sheet grades. With a melt flow rate of 4.0 g/10 min., MAGNUM AG700 can be used for low gloss, low impact applications where easy processability is desired.Data provided by Dow Chemical.This product line was spun off from Dow Chemical to Styron in 2010.
Physical Properties Metric English Comments
Density 1.04 g/cc
0.0376 lb/in³
ASTM Data
Linear Mold Shrinkage 0.0055 cm/cm
0.0055 in/in
Melt Flow 3.9 g/10 min

@Load 3.80 kg,
Temperature 230 °C
3.9 g/10 min

@Load 8.38 lb,
Temperature 446 °F
ASTM Data
Mechanical Properties Metric English Comments
Hardness, Rockwell R 108
108
Tensile Strength, Yield 30.3 MPa
4390 psi
ASTM Data
Elongation at Yield 1.8 %
1.8 %
ISO Data
Tensile Modulus 1.86 GPa
270 ksi
ASTM Data
Izod Impact, Notched 1.33 J/cm
2.49 ft-lb/in
ASTM Data
Charpy Impact Unnotched NB
NB
ISO Data
NB
NB
ISO Data, Low Temp
Charpy Impact, Notched 0.700 J/cm²
3.33 ft-lb/in²
ISO Data, Low Temp
1.60 J/cm²
7.61 ft-lb/in²
ISO Data
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 74.0 µm/m-°C

@Temperature 20.0 °C
41.1 µin/in-°F

@Temperature 68.0 °F
ISO data
Deflection Temperature at 1.8 MPa (264 psi) 98.9 °C
210 °F
Annealed; ASTM Data
Vicat Softening Point 104 °C
219 °F
Flammability, UL94 HB

@Thickness 1.47 mm
HB

@Thickness 0.0579 in