Styrolution Novodur® 4115 ABS

Category Polymer , Thermoplastic , ABS Polymer , Polycarbonate/ABS Alloy, Unreinforced , Polycarbonate (PC)
Manufacturer Styrolution
Trade Name Novodur®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Styrolution Novodur® 4115 ABS.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Novodur Ultra 4115 is a PC modified high heat injection molding grade. It provides good heat resistance combined with high impact strength.Information provided by Styrolution
Physical Properties Metric English Comments
Density 1.08 g/cc
0.0390 lb/in³
ISO 1183
Linear Mold Shrinkage 0.0060 - 0.0080 cm/cm
0.0060 - 0.0080 in/in
ISO 294-4
Melt Flow 6.0 g/10 min

@Load 10.0 kg,
Temperature 220 °C
6.0 g/10 min

@Load 22.0 lb,
Temperature 428 °F
ISO 1133
12 g/10 min

@Load 5.00 kg,
Temperature 260 °C
12 g/10 min

@Load 11.0 lb,
Temperature 500 °F
ISO 1133
Mechanical Properties Metric English Comments
Ball Indentation Hardness 100 MPa
14500 psi
ISO 2039-1
Tensile Strength, Yield 47.0 MPa
6820 psi
ISO 527
Elongation at Yield 3.8 %
3.8 %
ISO 527
Tensile Modulus 2.25 GPa
326 ksi
ISO 527
Flexural Strength 70.0 MPa
10200 psi
ISO 178
Flexural Modulus 2.20 GPa
319 ksi
ISO 178
Izod Impact, Notched (ISO) 12.0 kJ/m²

@Temperature -30.0 °C
5.71 ft-lb/in²

@Temperature -22.0 °F
ISO 180/A
40.0 kJ/m²

@Temperature 23.0 °C
19.0 ft-lb/in²

@Temperature 73.4 °F
ISO 180/A
Charpy Impact, Notched 1.30 J/cm²

@Temperature -30.0 °C
6.19 ft-lb/in²

@Temperature -22.0 °F
ISO 179
4.20 J/cm²

@Temperature 23.0 °C
20.0 ft-lb/in²

@Temperature 73.4 °F
ISO 179
Thermal Properties Metric English Comments
CTE, linear 80.0 µm/m-°C
44.4 µin/in-°F
ISO 11359
Deflection Temperature at 0.46 MPa (66 psi) 114 °C
237 °F
ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 103 °C
217 °F
ISO 75
Vicat Softening Point 116 °C

@Load 5.10 kg
241 °F

@Load 11.2 lb
50°C/h; ISO 306
Electrical Properties Metric English Comments
Volume Resistivity >= 1.00e+15 ohm-cm
>= 1.00e+15 ohm-cm
IEC 60093
Surface Resistance >= 1.00e+15 ohm
>= 1.00e+15 ohm
IEC 60093
Dielectric Constant 3.0

@Frequency 100 Hz
3.0

@Frequency 100 Hz
IEC 60250
Dielectric Strength 38.0 kV/mm

@Thickness 1.50 mm
965 kV/in

@Thickness 0.0591 in
Short Time; IEC 60243-1
Dissipation Factor 0.0045

@Frequency 100 Hz
0.0045

@Frequency 100 Hz
IEC 60250
0.0085

@Frequency 1.00e+6 Hz
0.0085

@Frequency 1.00e+6 Hz
IEC 60250
Comparative Tracking Index 600 V
600 V
IEC 60112
Processing Properties Metric English Comments
Melt Temperature 230 - 270 °C
446 - 518 °F
ISO 294
Mold Temperature 70.0 °C
158 °F
ISO 294
Injection Velocity 240 mm/sec
9.45 in/sec
ISO 294
Drying Temperature 80.0 °C

@Time 7200 - 14400 sec
176 °F

@Time 2.00 - 4.00 hour