Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gravity | 1.20 g/cc | 1.20 g/cc | ASTM D 792 |
Density | 1.20 g/cc | 0.0434 lb/in³ | ISO 1183 |
Moisture Absorption at Equilibrium | 0.80 % | 0.80 % | 23°C / 50% RH; ISO 62 |
Water Absorption at Saturation | 4.0 % @Temperature 23.0 °C |
4.0 % @Temperature 73.4 °F |
ISO 62 |
Linear Mold Shrinkage, Flow | 0.0050 - 0.0070 cm/cm | 0.0050 - 0.0070 in/in | on tensile bar; SABIC Method |
0.0050 - 0.0070 cm/cm @Thickness 3.20 mm |
0.0050 - 0.0070 in/in @Thickness 0.126 in |
SABIC Method | |
Linear Mold Shrinkage, Transverse | 0.0070 - 0.0090 cm/cm @Thickness 3.20 mm |
0.0070 - 0.0090 in/in @Thickness 0.126 in |
SABIC Method |
Melt Flow | 9.0 g/10 min @Load 2.16 kg, Temperature 280 °C |
9.0 g/10 min @Load 4.76 lb, Temperature 536 °F |
[cm^3/10 min] Melt Volume Rate; ISO 1133 |
39 g/10 min @Load 5.00 kg, Temperature 280 °C |
39 g/10 min @Load 11.0 lb, Temperature 536 °F |
ASTM D 1238 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Hardness, H358/30 | 130 MPa | 18900 psi | ISO 2039-1 |
Tensile Strength at Break | 83.0 MPa | 12000 psi | Type I, 5 mm/min; ASTM D 638 |
85.0 MPa | 12300 psi | 5 mm/min; ISO 527 | |
Tensile Strength, Yield | 90.0 MPa | 13100 psi | Type I, 5 mm/min; ASTM D 638 |
90.0 MPa | 13100 psi | 5 mm/min; ISO 527 | |
Elongation at Break | 6.0 % | 6.0 % | 5 mm/min; ISO 527 |
8.0 % | 8.0 % | Type I, 5 mm/min; ASTM D 638 | |
Elongation at Yield | 3.0 % | 3.0 % | 5 mm/min; ISO 527 |
5.0 % | 5.0 % | Type I, 5 mm/min; ASTM D 638 | |
Tensile Modulus | 4.30 GPa | 624 ksi | 5 mm/min; ASTM D 638 |
4.30 GPa | 624 ksi | 1 mm/min; ISO 527 | |
Flexural Yield Strength | 145 MPa | 21000 psi | 1.3 mm/min, 50 mm span; ASTM D 790 |
145 MPa | 21000 psi | 2 mm/min; ISO 178 | |
Flexural Modulus | 4.00 GPa | 580 ksi | 1.3 mm/min, 50 mm span; ASTM D 790 |
4.00 GPa | 580 ksi | 2 mm/min; ISO 178 | |
Izod Impact, Notched | 0.530 J/cm @Temperature 23.0 °C |
0.993 ft-lb/in @Temperature 73.4 °F |
ASTM D 256 |
Izod Impact, Unnotched | 5.87 J/cm @Temperature 23.0 °C |
11.0 ft-lb/in @Temperature 73.4 °F |
ASTM D 4812 |
Izod Impact, Notched (ISO) | 3.00 kJ/m² @Temperature -30.0 °C |
1.43 ft-lb/in² @Temperature -22.0 °F |
80*10*4; ISO 180/1A |
13.0 kJ/m² @Temperature 23.0 °C |
6.19 ft-lb/in² @Temperature 73.4 °F |
80*10*4; ISO 180/1A | |
Izod Impact, Unnotched (ISO) | 30.0 kJ/m² @Temperature -30.0 °C |
14.3 ft-lb/in² @Temperature -22.0 °F |
80*10*4; ISO 180/1U |
40.0 kJ/m² @Temperature 23.0 °C |
19.0 ft-lb/in² @Temperature 73.4 °F |
80*10*4; ISO 180/1U | |
Charpy Impact Unnotched | 3.50 J/cm² @Temperature -30.0 °C |
16.7 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*4 sp=62mm; ISO 179/1eU |
5.00 J/cm² @Temperature 23.0 °C |
23.8 ft-lb/in² @Temperature 73.4 °F |
Edgew 80*10*4 sp=62mm; ISO 179/1eU | |
Charpy Impact, Notched | 0.200 J/cm² @Temperature -30.0 °C |
0.952 ft-lb/in² @Temperature -22.0 °F |
V-notch Edgew 80*10*4 sp=62mm; ISO 179/1eA |
0.400 J/cm² @Temperature 23.0 °C |
1.90 ft-lb/in² @Temperature 73.4 °F |
V-notch Edgew 80*10*4 sp=62mm; ISO 179/1eA | |
Impact Test | 3.00 J @Temperature 23.0 °C |
2.21 ft-lb @Temperature 73.4 °F |
Instrumented Impact Total Energy; ASTM D 3763 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 54.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
30.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
55.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
30.6 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 | |
CTE, linear, Transverse to Flow | 90.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
50.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
100 µm/m-°C @Temperature 23.0 - 60.0 °C |
55.6 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 | |
Deflection Temperature at 0.46 MPa (66 psi) | 190 °C | 374 °F | Edgew 120*10*4 sp=100mm; ISO 75/Be |
239 °C | 462 °F | Flatw 80*10*4 sp=64mm; ISO 75/Bf | |
235 °C @Thickness 3.20 mm |
455 °F @Thickness 0.126 in |
unannealed; ASTM D 648 | |
Vicat Softening Point | 220 °C | 428 °F | Rate B/50; ASTM D 1525 |
230 °C | 446 °F | Rate B/50; ISO 306 | |
230 °C | 446 °F | Rate B/120; ISO 306 | |
UL RTI, Electrical | 120 °C | 248 °F | UL 746B |
UL RTI, Mechanical with Impact | 90.0 °C | 194 °F | UL 746B |
UL RTI, Mechanical without Impact | 95.0 °C | 203 °F | UL 746B |
Flammability, UL94 | V-1 @Thickness 1.00 mm |
V-1 @Thickness 0.0394 in |
UL 94 by SABIC-IP |
V-1 @Thickness 1.00 mm |
V-1 @Thickness 0.0394 in |
UL 94 | |
V-0 @Thickness 3.00 mm |
V-0 @Thickness 0.118 in |
UL 94 by SABIC-IP | |
V-0 @Thickness 3.00 mm |
V-0 @Thickness 0.118 in |
UL 94 | |
5VA @Thickness 2.50 mm |
5VA @Thickness 0.0984 in |
UL 94 by SABIC-IP | |
5VA @Thickness 2.50 mm |
5VA @Thickness 0.0984 in |
UL 94 | |
Oxygen Index | 33 % | 33 % | LOI; ISO 4589 |
Glow Wire Test | 850 °C @Thickness 1.60 mm |
1560 °F @Thickness 0.0630 in |
Glow Wire Flammability Index; IEC 60695-2-12 |
960 °C @Thickness 2.00 mm |
1760 °F @Thickness 0.0787 in |
Glow Wire Flammability Index; IEC 60695-2-12 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 1.20e+16 ohm-cm | 1.20e+16 ohm-cm | IEC 60093 |
Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | ROA; IEC 60093 |
Dielectric Constant | 3.0 @Frequency 1.00e+6 Hz |
3.0 @Frequency 1.00e+6 Hz |
IEC 60250 |
Dielectric Strength | 16.0 kV/mm @Thickness 3.20 mm |
406 kV/in @Thickness 0.126 in |
in oil; IEC 60243-1 |
22.0 kV/mm @Thickness 1.60 mm |
559 kV/in @Thickness 0.0630 in |
in oil; IEC 60243-1 | |
31.0 kV/mm @Thickness 0.800 mm |
787 kV/in @Thickness 0.0315 in |
in oil; IEC 60243-1 | |
Dissipation Factor | 0.018 @Frequency 1.00e+6 Hz |
0.018 @Frequency 1.00e+6 Hz |
IEC 60250 |
Comparative Tracking Index | 250 - 400 V | 250 - 400 V | PLC code 2; UL 746A |
375 V | 375 V | IEC 60112 | |
Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | PLC code 1; UL 746A |
High Amp Arc Ignition, HAI | >= 120 arcs | >= 120 arcs | surface, PLC code 0; UL 746A |
Descriptive Properties | Value | Comments |
---|---|---|
Ball Pressure Test, 125°C +/- 2°C | Pass | IEC 60695-10-2 |