Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate, Carbon + PTFE Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.27 - 1.50 g/cc
0.0459 - 0.0542 lb/in³
Average value: 1.36 g/cc Grade Count:57
Filler Content 10.0 - 40.0 %
10.0 - 40.0 %
Average value: 19.8 % Grade Count:29
Water Absorption 0.0600 - 0.310 %
0.0600 - 0.310 %
Average value: 0.118 % Grade Count:32
Additive Loading 10.0 - 15.0 %
10.0 - 15.0 %
Average value: 11.7 % Grade Count:3
Linear Mold Shrinkage 0.000 - 0.0100 cm/cm
0.000 - 0.0100 in/in
Average value: 0.00164 cm/cm Grade Count:50
Linear Mold Shrinkage, Transverse 0.000800 - 0.00500 cm/cm
0.000800 - 0.00500 in/in
Average value: 0.00373 cm/cm Grade Count:9
Mechanical Properties Metric English Comments
Hardness, Rockwell R 116 - 120
116 - 120
Average value: 118 Grade Count:5
Tensile Strength, Ultimate 89.6 - 193 MPa
13000 - 28000 psi
Average value: 121 MPa Grade Count:58
Tensile Strength, Yield 91.7 - 129 MPa
13300 - 18700 psi
Average value: 110 MPa Grade Count:7
Elongation at Break 1.00 - 10.0 %
1.00 - 10.0 %
Average value: 2.65 % Grade Count:54
Elongation at Yield 1.90 - 6.00 %
1.90 - 6.00 %
Average value: 2.97 % Grade Count:10
Modulus of Elasticity 6.89 - 24.1 GPa
999 - 3500 ksi
Average value: 12.3 GPa Grade Count:43
Flexural Yield Strength 121 - 255 MPa
17500 - 37000 psi
Average value: 181 MPa Grade Count:55
Flexural Modulus 6.21 - 21.7 GPa
900 - 3150 ksi
Average value: 11.2 GPa Grade Count:53
Izod Impact, Notched 0.427 - 3.50 J/cm
0.800 - 6.56 ft-lb/in
Average value: 0.972 J/cm Grade Count:56
Izod Impact, Unnotched 0.801 - 8.54 J/cm
1.50 - 16.0 ft-lb/in
Average value: 5.11 J/cm Grade Count:44
Izod Impact, Notched (ISO) 7.20 - 8.95 kJ/m²
3.43 - 4.26 ft-lb/in²
Average value: 8.05 kJ/m² Grade Count:5
Izod Impact, Unnotched (ISO) 22.0 - 34.0 kJ/m²
10.5 - 16.2 ft-lb/in²
Average value: 27.8 kJ/m² Grade Count:5
Charpy Impact Unnotched 3.00 - 4.50 J/cm²
14.3 - 21.4 ft-lb/in²
Average value: 3.50 J/cm² Grade Count:3
Falling Dart Impact 11.3 - 16.1 J
8.33 - 11.9 ft-lb
Average value: 13.5 J Grade Count:8
Coefficient of Friction 0.160 - 0.430
0.160 - 0.430
Average value: 0.253 Grade Count:3
Coefficient of Friction, Static 0.220 - 0.340
0.220 - 0.340
Average value: 0.267 Grade Count:3
K (wear) Factor 7.00 - 76.5 x 10<sup>-8</sup> mm³/N-M
3.47 - 38.0 x 10<sup>-10</sup> in³-min/ft-lb-hr
Average value: 30.8 x 10<sup>-8</sup> mm³/N-M Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 18.0 - 40.0 µm/m-°C
10.0 - 22.2 µin/in-°F
Average value: 28.8 µm/m-°C Grade Count:9
CTE, linear, Transverse to Flow 32.0 - 45.0 µm/m-°C
17.8 - 25.0 µin/in-°F
Average value: 38.0 µm/m-°C Grade Count:5
Deflection Temperature at 0.46 MPa (66 psi) 135 - 151 °C
275 - 304 °F
Average value: 145 °C Grade Count:32
Deflection Temperature at 1.8 MPa (264 psi) 132 - 149 °C
270 - 300 °F
Average value: 142 °C Grade Count:49
Vicat Softening Point 147 - 150 °C
297 - 302 °F
Average value: 149 °C Grade Count:3
Flammability, UL94 HB - V-0
HB - V-0
Grade Count:39
Electrical Properties Metric English Comments
Electrical Resistivity 1.00 - 1.00e+7 ohm-cm
1.00 - 1.00e+7 ohm-cm
Average value: 160000 ohm-cm Grade Count:39
Surface Resistance 10.0 - 1.00e+7 ohm
10.0 - 1.00e+7 ohm
Average value: 797000 ohm Grade Count:21
Processing Properties Metric English Comments
Processing Temperature 249 - 293 °C
480 - 560 °F
Average value: 271 °C Grade Count:15
Nozzle Temperature 271 - 316 °C
520 - 601 °F
Average value: 293 °C Grade Count:8
Melt Temperature 254 - 327 °C
489 - 621 °F
Average value: 296 °C Grade Count:36
Mold Temperature 48.9 - 121 °C
120 - 250 °F
Average value: 91.4 °C Grade Count:51
Drying Temperature 110 - 130 °C
230 - 266 °F
Average value: 121 °C Grade Count:36
Moisture Content 0.0200 %
0.0200 %
Average value: 0.0200 % Grade Count:32
Dew Point -28.9 °C
-20.0 °F
Average value: -28.9 °C Grade Count:17
Injection Pressure 68.9 - 103 MPa
10000 - 15000 psi
Average value: 86.2 MPa Grade Count:32
Vent Depth 0.00250 - 0.00760 cm
0.000984 - 0.00299 in
Average value: 0.00505 cm Grade Count:8
Users viewing this material also viewed the following: