| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.14 g/cc | 0.0412 lb/in³ | DAM; ISO 1183 |
| Water Absorption | 8.5 % @Thickness 2.00 mm |
8.5 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Moisture Absorption | 2.60 % @Thickness 2.00 mm |
2.60 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0090 cm/cm | 0.0090 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.012 cm/cm | 0.012 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Stress | 14.8 MPa @Strain 0.430 %, Temperature 23.0 °C |
2150 psi @Strain 0.430 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 |
| 17.92 MPa @Strain 5.00 %, Temperature 150 °C |
2599 psi @Strain 5.00 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 18.65 MPa @Strain 0.510 %, Temperature 0.000 °C |
2705 psi @Strain 0.510 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 27.93 MPa @Strain 0.710 %, Temperature -40.0 °C |
4051 psi @Strain 0.710 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 29.51 MPa @Strain 20.0 %, Temperature 150 °C |
4280 psi @Strain 20.0 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 68.03 MPa @Strain 2.15 %, Temperature 23.0 °C |
9867 psi @Strain 2.15 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 68.75 MPa @Strain 2.04 %, Temperature 0.000 °C |
9971 psi @Strain 2.04 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 88.64 MPa @Strain 3.44 %, Temperature 23.0 °C |
12860 psi @Strain 3.44 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 94.93 MPa @Strain 2.83 %, Temperature -40.0 °C |
13770 psi @Strain 2.83 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 100.6 MPa @Strain 3.56 %, Temperature 0.000 °C |
14590 psi @Strain 3.56 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 106.32 MPa @Strain 5.09 %, Temperature 0.000 °C |
15420 psi @Strain 5.09 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 128.87 MPa @Strain 4.96 %, Temperature -40.0 °C |
18691 psi @Strain 4.96 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 135.06 MPa @Strain 7.09 %, Temperature -40.0 °C |
19589 psi @Strain 7.09 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| Tensile Strength, Yield | 60.0 MPa | 8700 psi | 50%RH; ISO 527-1/-2 |
| 91.0 MPa | 13200 psi | DAM; ISO 527-1/-2 | |
| Elongation at Break | 13 % | 13 % | DAM; Nominal; ISO 527-1/-2 |
| >= 50 % | >= 50 % | 50%RH; Nominal; ISO 527-1/-2 | |
| Elongation at Yield | 4.4 % | 4.4 % | DAM; ISO 527-3 |
| 4.5 % | 4.5 % | DAM; ISO 527-1/-2 | |
| 22 % | 22 % | 50%RH; ISO 527-1/-2 | |
| Tensile Modulus | 1.60 GPa | 232 ksi | 50%RH; ISO 527-1/-2 |
| 3.40 GPa | 493 ksi | DAM; ISO 527-1/-2 | |
| Flexural Modulus | 1.40 GPa | 203 ksi | 50%RH; ISO 178 |
| 3.00 GPa | 435 ksi | DAM; ISO 178 | |
| Shear Modulus | 0.175 GPa @Temperature 140 °C |
25.4 ksi @Temperature 284 °F |
DAM; Dynamic; ISO 11403-1 -2 |
| 0.280 GPa @Temperature 90.0 °C |
40.6 ksi @Temperature 194 °F |
DAM; Dynamic; ISO 11403-1 -2 | |
| 1.10 GPa @Temperature 40.0 °C |
160 ksi @Temperature 104 °F |
DAM; Dynamic; ISO 11403-1 -2 | |
| 1.18 GPa @Temperature 10.0 °C |
171 ksi @Temperature 50.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |
| 1.25 GPa @Temperature -20.0 °C |
181 ksi @Temperature -4.00 °F |
DAM; Dynamic; ISO 11403-1 -2 | |
| Secant Modulus | 0.233 GPa @Strain 16.51 %, Temperature 100 °C |
33.8 ksi @Strain 16.51 %, Temperature 212 °F |
DAM; ISO 11403-1 -2 |
| 0.489 GPa @Strain 4.13 %, Temperature 100 °C |
71.0 ksi @Strain 4.13 %, Temperature 212 °F |
DAM; ISO 11403-1 -2 | |
| 2.32 GPa @Strain 3.87 %, Temperature 23.0 °C |
336 ksi @Strain 3.87 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 2.3388 GPa @Strain 5.67 %, Temperature -40.0 °C |
339.22 ksi @Strain 5.67 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 2.5629 GPa @Strain 4.07 %, Temperature 0.000 °C |
371.72 ksi @Strain 4.07 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 3.16 GPa @Strain 2.15 %, Temperature 23.0 °C |
459 ksi @Strain 2.15 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 3.35 GPa @Strain 2.83 %, Temperature -40.0 °C |
487 ksi @Strain 2.83 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 3.3701 GPa @Strain 2.04 %, Temperature 0.000 °C |
488.80 ksi @Strain 2.04 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 3.44 GPa @Strain 0.430 %, Temperature 23.0 °C |
499 ksi @Strain 0.430 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 3.66 GPa @Strain 0.510 %, Temperature 0.000 °C |
530 ksi @Strain 0.510 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 3.9338 GPa @Strain 0.710 %, Temperature -40.0 °C |
570.56 ksi @Strain 0.710 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| Izod Impact, Notched (ISO) | 4.00 kJ/m² | 1.90 ft-lb/in² | DAM; ISO 180/1A |
| 8.00 kJ/m² | 3.81 ft-lb/in² | 50%RH; ISO 180/1A | |
| 2.00 kJ/m² @Temperature -30.0 °C |
0.952 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1A | |
| 4.00 kJ/m² @Temperature -30.0 °C |
1.90 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1A | |
| Izod Impact, Unnotched (ISO) | 300 kJ/m² | 143 ft-lb/in² | DAM; ISO 180/1U |
| NB | NB | 50%RH; ISO 180/1U | |
| Charpy Impact Unnotched | 30.0 J/cm² | 143 ft-lb/in² | DAM; ISO 179/1eU |
| NB | NB | 50%RH; ISO 179/1eU | |
| 20.0 J/cm² @Temperature -30.0 °C |
95.2 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU | |
| Charpy Impact, Notched | 0.400 J/cm² | 1.90 ft-lb/in² | DAM; ISO 179/1eA |
| 0.800 J/cm² | 3.81 ft-lb/in² | 50%RH; ISO 179/1eA | |
| 0.250 J/cm² @Temperature -30.0 °C |
1.19 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA | |
| 0.350 J/cm² @Temperature -30.0 °C |
1.67 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 262 °C | 504 °F | DAM; 10°C/min; ISO 11357-1/-3 |
| Deflection Temperature at 0.46 MPa (66 psi) | 225 °C | 437 °F | DAM; ISO 75-1/-2 |
| Deflection Temperature at 1.8 MPa (264 psi) | 75.0 °C | 167 °F | DAM; ISO 75-1/-2 |
| Glass Transition Temp, Tg | 60.0 °C | 140 °F | DAM; 10°C/min; ISO 11357-1/-2 |
| Flammability, UL94 | V-2 @Thickness 1.50 mm |
V-2 @Thickness 0.0591 in |
DAM; IEC 60695-11-10 |
| V-2 @Thickness 0.700 mm |
V-2 @Thickness 0.0276 in |
DAM; IEC 60695-11-10 | |
| Oxygen Index | 29 % | 29 % | DAM; ISO 4589-1/-2 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Additives | Lubricants | |
| Release agent | ||
| Delivery Form | Pellets | |
| Part Marking Code | >PA66< | ISO 11469 |
| Processing | Injection Moulding | |
| Regional Availability | Asia Pacific | |
| Europe | ||
| Global | ||
| Near East/Africa | ||
| North America | ||
| South and Central America | ||
| Resin Identification | PA66 | |