Material Notes:
Description: AKROMID B3 GF 30 RM-M natural (3291) is a 30% glass fiber reinforced polyamide 6 with high stiffness and strength, limited moisture absorption and light inherent color.Applications: Applications are housings and other dimensional stable parts in the automotive and electronic industryInformation from Akro-Plastic
Physical Properties Metric English Comments
Density 1.41 g/cc
0.0509 lb/in³
ISO 1183
Filler Content 30 %
30 %
ISO 1172
Water Absorption 1.65 %

@Temperature 70.0 °C
1.65 %

@Temperature 158 °F
62% RH. Humidity; ISO 1110
Linear Mold Shrinkage, Flow 0.0030 cm/cm
0.0030 in/in
ISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
0.0080 in/in
ISO 294-4
Mechanical Properties Metric English Comments
Tensile Strength at Break 110 MPa
16000 psi
5 [mm/min]; ISO 527-2/5
Elongation at Break 4.5 %
4.5 %
5 [mm/min]; ISO 527-2/5
Tensile Modulus 7.10 GPa
1030 ksi
1 [mm/min]; ISO 527-1/2
Charpy Impact Unnotched 6.00 J/cm²

@Temperature -30.0 °C
28.6 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eU
7.00 J/cm²

@Temperature 23.0 °C
33.3 ft-lb/in²

@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 1.00 J/cm²

@Temperature -30.0 °C
4.76 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eA
1.50 J/cm²

@Temperature 23.0 °C
7.14 ft-lb/in²

@Temperature 73.4 °F
ISO 179/1eA