Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Eastman 5269 LDPE 6.5% EVA Copolymer, Clarity, Ultra-high Impact Film Resin  (discontinued **)

Category Polymer , Film , Thermoplastic , Ethylene Vinyl Acetate , Ethylene Vinyl Acetate Copolymer (EVA), Film Grade
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Eastman 5269 LDPE 6.5% EVA Copolymer, Clarity, Ultra-high Impact Film Resin  (discontinued **).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Resin Type: CopolymerCharacteristics: Medium Molecular Weight Distribution, Reduced Yellow Potential, Wide Range of Processing Conditions, Good Flow for Injection Blow Molding Applications, Good Parison Uniformity, Good TrimabilityApplications:Food Packaging, Personal Care Products, Coolers, Ice Chests, Sheet and Vacuum Forming, Oil BottlesProcessing Conditions: Extruder 6.35 cm. Screw L/D Ratio 24:1. Die Opening 0.0762 cm. Blow-Up Ratio 2:1.Film properties below based on film thickness of 31.8 µm.Eastman Chemical Company sold its polyethylene business to Westlake Chemical Corporation in Dec. 2006. This grade no longer appears in the Westlake product line.
Physical Properties Metric English Comments
Density 0.928 g/cc
0.0335 lb/in³
ASTM D1505
Melt Flow 0.50 g/10 min
0.50 g/10 min
Condition E; ASTM D 1238
Mechanical Properties Metric English Comments
Secant Modulus, MD 0.110 GPa
16.0 ksi
ASTM D882
Secant Modulus, TD 0.120 GPa
17.4 ksi
ASTM D882
Coefficient of Friction 1.0
1.0
ASTM D1894
Dart Drop 6.00 g/micron
152 g/mil
F<sub>50</sub>; 1.5 in. dart/26 in. drop height; ASTM D 1709
Optical Properties Metric English Comments
Haze 9.0 %
9.0 %
ASTM D2457
Gloss 47 %
47 %
at 45°. ASTM D 2457
75 %
75 %
at 60°. ASTM D 2457
Transmission, Visible 90 %
90 %
clear; thickness not quantified
Processing Properties Metric English Comments
Melt Temperature 204 °C
399 °F
Users viewing this material also viewed the following: