Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gravity | 1.42 g/cc | 1.42 g/cc | ASTM D792 |
Water Absorption | 0.19 % @Time 86400 sec |
0.19 % @Time 24.0 hour |
ASTM D570 |
Moisture Absorption at Equilibrium | 1.1 % | 1.1 % | ASTM D570 |
Linear Mold Shrinkage, Flow | 0.0030 - 0.0050 cm/cm @Thickness 3.20 mm |
0.0030 - 0.0050 in/in @Thickness 0.126 in |
SABIC Method |
Melt Flow | 6.0 g/10 min @Load 6.60 kg, Temperature 337 °C |
6.0 g/10 min @Load 14.6 lb, Temperature 639 °F |
ASTM D1238 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Hardness, Rockwell M | 114 | 114 | ASTM D785 |
Tensile Strength at Break | 131 MPa | 19000 psi | Type I, 5 mm/min; ASTM D638 |
Elongation at Break | 4.0 % | 4.0 % | Type I, 5 mm/min; ASTM D638 |
Tensile Modulus | 6.89 GPa | 999 ksi | 5 mm/min; ASTM D638 |
Flexural Strength | 227 MPa | 32900 psi | 2.6 mm/min, 100 mm span; ASTM D790 |
Flexural Modulus | 6.89 GPa | 999 ksi | 2.6 mm/min, 100 mm span; ASTM D790 |
Izod Impact, Notched | 0.640 J/cm | 1.20 ft-lb/in | ASTM D256 |
4.64 J/cm @Thickness 3.20 mm |
8.69 ft-lb/in @Thickness 0.126 in |
ASTM D256 | |
Izod Impact, Unnotched | 4.80 J/cm | 8.99 ft-lb/in | ASTM D4812 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 25.2 µm/m-°C @Temperature -20.0 - 150 °C |
14.0 µin/in-°F @Temperature -4.00 - 302 °F |
ASTM E 831 |
Deflection Temperature at 0.46 MPa (66 psi) | 210 °C @Thickness 6.40 mm |
410 °F @Thickness 0.252 in |
unannealed; ASTM D648 |
Deflection Temperature at 1.8 MPa (264 psi) | 210 °C @Thickness 6.40 mm |
410 °F @Thickness 0.252 in |
unannealed; ASTM D648 |
Vicat Softening Point | 220 °C | 428 °F | Rate B/50; ASTM D1525 |
Glass Transition Temp, Tg | 217 °C | 423 °F | |
UL RTI, Electrical | 170 °C | 338 °F | UL 746B |
UL RTI, Mechanical with Impact | 170 °C | 338 °F | UL 746B |
UL RTI, Mechanical without Impact | 170 °C | 338 °F | UL 746B |
Flammability, UL94 | V-0 @Thickness 0.400 mm |
V-0 @Thickness 0.0157 in |
UL 94 |
5VA @Thickness 1.90 mm |
5VA @Thickness 0.0748 in |
UL 94 | |
Oxygen Index | 50 % | 50 % | ASTM D2863 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 7.00e+16 ohm-cm | 7.00e+16 ohm-cm | ASTM D257 |
Dielectric Constant | 3.5 @Frequency 1000 Hz |
3.5 @Frequency 1000 Hz |
ASTM D150 |
Dielectric Strength | 26.3 kV/mm @Thickness 1.60 mm |
668 kV/in @Thickness 0.0630 in |
in oil; ASTM D149 |
Dissipation Factor | 0.0015 @Frequency 1000 Hz |
0.0015 @Frequency 1000 Hz |
ASTM D150 |
0.0049 @Frequency 2.45e+9 Hz |
0.0049 @Frequency 2.45e+9 Hz |
ASTM D150 | |
Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten; ASTM D495 |
Comparative Tracking Index | 100 - 175 V | 100 - 175 V | UL 746A |
Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | UL 746A |
High Amp Arc Ignition, HAI | 0.00 - 15 arcs | 0.00 - 15 arcs | UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80.0 mm/min | 1.00 - 3.15 in/min | UL 746A |
Descriptive Properties | Value | Comments |
---|---|---|
NBS Smoke Density, Flaming, Ds 4 min | 1.3 | ASTM E 662 |