| Category | Polymer , Thermoplastic , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | Lexan® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | SABIC Innovative Plastics Lexan® FXG1414T PC Copolymer (Europe-Africa-Middle East).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.18 g/cc | 1.18 g/cc | ASTM D 792 |
| Density | 1.18 g/cc | 0.0426 lb/in³ | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.090 % | 0.090 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.13 % <br>@Temperature 23.0 °C |
0.13 % <br>@Temperature 73.4 °F |
ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0080 cm/cm | 0.0040 - 0.0080 in/in | on tensile bar; SABIC Method |
| 0.0040 - 0.0080 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0080 in/in <br>@Thickness 0.126 in |
SABIC Method | |
| Linear Mold Shrinkage, Transverse | 0.0040 - 0.0080 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0080 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Melt Flow | 9.0 g/10 min <br>@Load 1.20 kg,<br> Temperature 300 °C |
9.0 g/10 min <br>@Load 2.65 lb,<br> Temperature 572 °F |
[cm^3/10 min] Melt Volume Rate; ISO 1133 |
| 10 g/10 min <br>@Load 1.20 kg,<br> Temperature 300 °C |
10 g/10 min <br>@Load 2.65 lb,<br> Temperature 572 °F |
ASTM D 1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 45.0 MPa | 6530 psi | Type I, 50 mm/min; ASTM D 638 |
| 49.0 MPa | 7110 psi | 50 mm/min; ISO 527 | |
| Tensile Strength, Yield | 56.0 MPa | 8120 psi | 50 mm/min; ISO 527 |
| 58.0 MPa | 8410 psi | Type I, 50 mm/min; ASTM D 638 | |
| Elongation at Break | 11.3 % | 11.3 % | 50 mm/min; ISO 527 |
| 52 % | 52 % | Type I, 50 mm/min; ASTM D 638 | |
| Elongation at Yield | 5.4 % | 5.4 % | 50 mm/min; ISO 527 |
| 5.7 % | 5.7 % | Type I, 50 mm/min; ASTM D 638 | |
| Tensile Modulus | 2.06 GPa | 299 ksi | 50 mm/min; ASTM D 638 |
| 2.25 GPa | 326 ksi | 1 mm/min; ISO 527 | |
| Flexural Yield Strength | 84.0 MPa | 12200 psi | 1.3 mm/min, 50 mm span; ASTM D 790 |
| 88.0 MPa | 12800 psi | 2 mm/min; ISO 178 | |
| Flexural Modulus | 2.15 GPa | 312 ksi | 2 mm/min; ISO 178 |
| 2.23 GPa | 323 ksi | 1.3 mm/min, 50 mm span; ASTM D 790 | |
| Izod Impact, Notched | 3.47 J/cm <br>@Temperature -30.0 °C |
6.50 ft-lb/in <br>@Temperature -22.0 °F |
ASTM D 256 |
| 5.23 J/cm <br>@Temperature 23.0 °C |
9.80 ft-lb/in <br>@Temperature 73.4 °F |
ASTM D 256 | |
| Impact Test | 49.0 J <br>@Temperature 23.0 °C |
36.1 ft-lb <br>@Temperature 73.4 °F |
Instrumented Impact Total Energy; ASTM D 3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 67.0 µm/m-°C <br>@Temperature 23.0 - 80.0 °C |
37.2 µin/in-°F <br>@Temperature 73.4 - 176 °F |
ISO 11359-2 |
| 67.0 µm/m-°C <br>@Temperature -40.0 - 95.0 °C |
37.2 µin/in-°F <br>@Temperature -40.0 - 203 °F |
ASTM E 831 | |
| CTE, linear, Transverse to Flow | 80.0 µm/m-°C <br>@Temperature 23.0 - 80.0 °C |
44.4 µin/in-°F <br>@Temperature 73.4 - 176 °F |
ISO 11359-2 |
| 80.0 µm/m-°C <br>@Temperature -40.0 - 95.0 °C |
44.4 µin/in-°F <br>@Temperature -40.0 - 203 °F |
ASTM E 831 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 117 °C | 243 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 121 °C <br>@Thickness 3.20 mm |
250 °F <br>@Thickness 0.126 in |
unannealed; ASTM D 648 | |
| Vicat Softening Point | 139 °C | 282 °F | Rate B/50; ASTM D 1525 |
| 139 °C | 282 °F | Rate B/50; ISO 306 | |
| 142 °C | 288 °F | Rate B/120; ISO 306 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Ball Pressure Test, 75°C +/- 2°C | PASS | IEC 60695-10-2 |