| Category | Polymer , Thermoplastic , ABS Polymer , Polycarbonate/ABS Alloy, Unreinforced , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | Cycoloy® |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | SABIC Innovative Plastics Cycoloy® CY5000 PC+ABS.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.18 g/cc | 1.18 g/cc | ASTM D792 |
| Density | 1.18 g/cc | 0.0426 lb/in³ | ISO 1183 |
| Moisture Absorption | 0.0500 % | 0.0500 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.10 % | 0.10 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0060 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0060 in/in @Thickness 0.126 in |
SABIC Method |
| Melt Flow | 34 g/10 min @Load 2.16 kg, Temperature 260 °C |
34 g/10 min @Load 4.76 lb, Temperature 500 °F |
ASTM D1238 |
| Melt Index of Compound | 30 g/10 min @Load 2.16 kg, Temperature 260 °C |
30 g/10 min @Load 4.76 lb, Temperature 500 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 43.0 MPa | 6240 psi | 50 mm/min; ISO 527 |
| 48.0 MPa | 6960 psi | Type I, 50 mm/min; ASTM D638 | |
| Tensile Strength, Yield | 63.0 MPa | 9140 psi | 50 mm/min; ISO 527 |
| 65.0 MPa | 9430 psi | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Break | 34 % | 34 % | Type I, 50 mm/min; ASTM D638 |
| 40 % | 40 % | 50 mm/min; ISO 527 | |
| Elongation at Yield | 3.5 % | 3.5 % | 50 mm/min; ISO 527 |
| 3.9 % | 3.9 % | Type I, 50 mm/min; ASTM D638 | |
| Tensile Modulus | 2.67 GPa | 387 ksi | 1 mm/min; ISO 527 |
| 2.80 GPa | 406 ksi | 5 mm/min; ASTM D638 | |
| Flexural Yield Strength | 95.0 MPa | 13800 psi | 2 mm/min; ISO 178 |
| 97.0 MPa | 14100 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 2.63 GPa | 381 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
| 2.70 GPa | 392 ksi | 2 mm/min; ISO 178 | |
| Izod Impact, Notched | 0.900 J/cm | 1.69 ft-lb/in | ASTM D256 |
| 0.690 J/cm @Temperature -30.0 °C |
1.29 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 10.0 kJ/m² | 4.76 ft-lb/in² | 80*10*3; ISO 180/1A |
| 5.00 kJ/m² @Temperature -30.0 °C |
2.38 ft-lb/in² @Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
| Charpy Impact, Notched | 1.00 J/cm² | 4.76 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
| 0.500 J/cm² @Temperature -30.0 °C |
2.38 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 20.0 J @Temperature 23.0 °C |
14.8 ft-lb @Temperature 73.4 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 71.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
39.4 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 |
| 73.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
40.6 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 | |
| CTE, linear, Transverse to Flow | 72.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
40.0 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 |
| 78.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
43.3 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 73.0 °C | 163 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 81.0 °C @Thickness 6.40 mm |
178 °F @Thickness 0.252 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 89.0 °C | 192 °F | Rate B/50; ISO 306 |
| 92.0 °C | 198 °F | Rate B/120; ISO 306 | |
| Flammability, UL94 | V-1 @Thickness 1.50 mm |
V-1 @Thickness 0.0591 in |
UL 94 |
| V-0 @Thickness 2.00 mm |
V-0 @Thickness 0.0787 in |
UL 94 |