Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

EMS-Grivory Grivory® TR 55 LX PA12/MACMI

Category Polymer , Thermoplastic , Nylon , Nylon 12
Manufacturer EMS-Grivory (EMS-CHEMIE)
Trade Name Grivory®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF EMS-Grivory Grivory® TR 55 LX PA12/MACMI.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Product description: Grilamid TR 55 LX natural is a high purity transparent thermoplastic polyamide, based on aliphatic and cycloaliphatic monomers. Grilamid TR 55 LX natural offers outstanding properties such as:Transparency and weathering stabilityUnlimited colorabilityStress crack resistanceToughness and stiffnessVery good chemical resistance Grilamid TR 55 LX natural is especially suited for injection molded out door applications in the application fields of: OpticsAutomotiveMechanical engineeringSafety technologySport & LeisureInformation provided by EMS Grivory
Physical Properties Metric English Comments
Density 1.04 g/cc
0.0376 lb/in³
ISO 1183
Water Absorption 2.5 %
2.5 %
ISO 62
Moisture Absorption 1.00 %
1.00 %
ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cm
0.0050 in/in
ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0060 cm/cm
0.0060 in/in
ISO 294-4, 2577
Mechanical Properties Metric English Comments
Ball Indentation Hardness 110 MPa
16000 psi
conditioned; ISO 2039-1
Tensile Strength at Break 40.0 MPa
5800 psi
conditioned; ISO 527-1/-2
Tensile Strength, Yield 70.0 MPa
10200 psi
conditioned; ISO 527-1/-2
Elongation at Break >= 50 %
>= 50 %
conditioned; ISO 527-1/-2
Elongation at Yield 6.0 %
6.0 %
conditioned; ISO 527-1/-2
Tensile Modulus 1.90 GPa
276 ksi
conditioned; ISO 527-1/-2
Charpy Impact Unnotched NB
NB
conditioned; ISO 179/1eU
NB

@Temperature 30.0 °C
NB

@Temperature 86.0 °F
conditioned; ISO 179/1eU
Charpy Impact, Notched 0.900 J/cm²
4.28 ft-lb/in²
conditioned; ISO 179/1eA
0.800 J/cm²

@Temperature 30.0 °C
3.81 ft-lb/in²

@Temperature 86.0 °F
conditioned; ISO 179/1eU
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 90.0 µm/m-°C
50.0 µin/in-°F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C
50.0 µin/in-°F
ISO 11359-1/-2
Maximum Service Temperature, Air 80.0 °C
176 °F
long term; EMS
95.0 °C
203 °F
short term; EMS
Transformation Temperature, Tg 110 °C
230 °F
10°C/min; ISO 11357-1/-2
Deflection Temperature at 0.46 MPa (66 psi) 90.0 °C
194 °F
ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C
176 °F
ISO 75-1/-2
Flammability, UL94 HB
HB
IEC 60695-11-10
Optical Properties Metric English Comments
Transmission, Visible 90 %
90 %
transparent; thickness not quantified
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+13 ohm-cm
1.00e+13 ohm-cm
conditioned; IEC 60093
Surface Resistance 1.00e+12 ohm
1.00e+12 ohm
IEC 60093
Dielectric Strength 32.0 kV/mm
813 kV/in
conditioned; IEC 60243-1
Comparative Tracking Index 600 V
600 V
conditioned; IEC 60112
Descriptive Properties Value Comments
Automotive Automotive electr. and electronics, lighting
Cooling and climate control
Fuel systems
Interior
Powertrain and Chassis
Electricals & Electronics Cables & Tubes
Electrical appliances
Electrical equipment
Energy distribution
Lighting
Mobile phones and other portable devices
Form Granules
Industry & Consumer goods Housewares
Hydraulics & Pneumatics
Mechanical Engineering
Medical devices
Power transmission
Sanitary, water and gas supply
Sports & Leisure
Tools & Accessories
Optics Optical components
Spectacle frames
Sunglasses
Processing Injection Molding
Product Attributes Improved alcohol resistance
Special Characteristics Transparent
Water Contact NSF 61