| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.19 g/cc | 0.0430 lb/in³ | |
| 1.42 g/cc | 0.0513 lb/in³ | ISO 1183 | |
| Viscosity | 135800 cP <br>@Shear Rate 5000 1/s,<br> Temperature 230 °C |
135800 cP <br>@Shear Rate 5000 1/s,<br> Temperature 446 °F |
ISO 11403-1 -2 |
| 156200 cP <br>@Shear Rate 5000 1/s,<br> Temperature 215 °C |
156200 cP <br>@Shear Rate 5000 1/s,<br> Temperature 419 °F |
ISO 11403-1 -2 | |
| 164900 cP <br>@Shear Rate 5000 1/s,<br> Temperature 200 °C |
164900 cP <br>@Shear Rate 5000 1/s,<br> Temperature 392 °F |
ISO 11403-1 -2 | |
| 678700 cP <br>@Shear Rate 500 1/s,<br> Temperature 230 °C |
678700 cP <br>@Shear Rate 500 1/s,<br> Temperature 446 °F |
ISO 11403-1 -2 | |
| 697510 cP <br>@Shear Rate 500 1/s,<br> Temperature 215 °C |
697510 cP <br>@Shear Rate 500 1/s,<br> Temperature 419 °F |
ISO 11403-1 -2 | |
| 769600 cP <br>@Shear Rate 500 1/s,<br> Temperature 200 °C |
769600 cP <br>@Shear Rate 500 1/s,<br> Temperature 392 °F |
ISO 11403-1 -2 | |
| Linear Mold Shrinkage, Flow | 0.022 cm/cm | 0.022 in/in | ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.018 cm/cm | 0.018 in/in | ISO 294-4 2577 |
| Melt Flow | 1.9 g/10 min <br>@Load 2.16 kg,<br> Temperature 190 °C |
1.9 g/10 min <br>@Load 4.76 lb,<br> Temperature 374 °F |
cm³/10min; ISO 1133 |
| 2.2 g/10 min <br>@Load 2.16 kg,<br> Temperature 190 °C |
2.2 g/10 min <br>@Load 4.76 lb,<br> Temperature 374 °F |
ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 91 | 91 | ISO 2039-2 |
| Hardness, Rockwell R | 121 | 121 | ISO 2039-2 |
| Tensile Stress | 7.10 MPa <br>@Strain 0.500 %,<br> Temperature 90.0 °C |
1030 psi <br>@Strain 0.500 %,<br> Temperature 194 °F |
ISO 11403-1 -2 |
| 21.4 MPa <br>@Strain 2.10 %,<br> Temperature 90.0 °C |
3100 psi <br>@Strain 2.10 %,<br> Temperature 194 °F |
ISO 11403-1 -2 | |
| 29.0 MPa <br>@Strain 3.70 %,<br> Temperature 90.0 °C |
4210 psi <br>@Strain 3.70 %,<br> Temperature 194 °F |
ISO 11403-1 -2 | |
| 31.3 MPa <br>@Strain 1.10 %,<br> Temperature 23.0 °C |
4540 psi <br>@Strain 1.10 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 31.9 MPa <br>@Strain 5.00 %,<br> Temperature 90.0 °C |
4630 psi <br>@Strain 5.00 %,<br> Temperature 194 °F |
ISO 11403-1 -2 | |
| 53.9 MPa <br>@Strain 2.40 %,<br> Temperature 0.000 °C |
7820 psi <br>@Strain 2.40 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 60.4 MPa <br>@Strain 1.70 %,<br> Temperature -40.0 °C |
8760 psi <br>@Strain 1.70 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 62.0 MPa <br>@Strain 4.50 %,<br> Temperature 23.0 °C |
8990 psi <br>@Strain 4.50 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 66.1 MPa <br>@Strain 7.00 %,<br> Temperature 23.0 °C |
9590 psi <br>@Strain 7.00 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 68.0 MPa <br>@Strain 11.0 %,<br> Temperature 23.0 °C |
9860 psi <br>@Strain 11.0 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 76.5 MPa <br>@Strain 9.00 %,<br> Temperature 0.000 °C |
11100 psi <br>@Strain 9.00 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 78.9 MPa <br>@Strain 17.0 %,<br> Temperature 0.000 °C |
11400 psi <br>@Strain 17.0 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 79.7 MPa <br>@Strain 24.0 %,<br> Temperature 0.000 °C |
11600 psi <br>@Strain 24.0 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 93.0 MPa <br>@Strain 6.00 %,<br> Temperature -40.0 °C |
13500 psi <br>@Strain 6.00 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 96.0 MPa <br>@Strain 11.0 %,<br> Temperature -40.0 °C |
13900 psi <br>@Strain 11.0 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 97.6 MPa <br>@Strain 18.0 %,<br> Temperature -40.0 °C |
14200 psi <br>@Strain 18.0 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| Tensile Strength, Yield | 72.0 MPa | 10400 psi | ISO 527-1/-2 |
| Elongation at Break | >= 50 % | >= 50 % | Nominal; ISO 527-1/-2 |
| Elongation at Yield | 23 % | 23 % | ISO 527-1/-2 |
| Tensile Modulus | 3.15 GPa | 457 ksi | ISO 527-1/-2 |
| Flexural Modulus | 0.0800 GPa | 11.6 ksi | ASTM D790 |
| 2.90 GPa | 421 ksi | ISO 178 | |
| Secant Modulus | 0.276 GPa <br>@Strain 29.0 %,<br> Temperature 0.000 °C |
40.1 ksi <br>@Strain 29.0 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 |
| 0.303 GPa <br>@Strain 32.5 %,<br> Temperature -40.0 °C |
43.9 ksi <br>@Strain 32.5 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 0.321 GPa <br>@Strain 21.4 %,<br> Temperature 23.0 °C |
46.6 ksi <br>@Strain 21.4 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 0.417 GPa <br>@Strain 19.0 %,<br> Temperature 0.000 °C |
60.5 ksi <br>@Strain 19.0 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 0.426 GPa <br>@Strain 23.0 %,<br> Temperature -40.0 °C |
61.7 ksi <br>@Strain 23.0 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 0.526 GPa <br>@Strain 13.0 %,<br> Temperature 23.0 °C |
76.3 ksi <br>@Strain 13.0 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 0.744 GPa <br>@Strain 13.0 %,<br> Temperature -40.0 °C |
108 ksi <br>@Strain 13.0 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 0.749 GPa <br>@Strain 9.00 %,<br> Temperature 23.0 °C |
109 ksi <br>@Strain 9.00 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 0.850 GPa <br>@Strain 9.00 %,<br> Temperature 0.000 °C |
123 ksi <br>@Strain 9.00 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 1.38 GPa <br>@Strain 4.50 %,<br> Temperature 23.0 °C |
200 ksi <br>@Strain 4.50 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 1.55 GPa <br>@Strain 6.00 %,<br> Temperature -40.0 °C |
225 ksi <br>@Strain 6.00 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 2.25 GPa <br>@Strain 2.40 %,<br> Temperature 0.000 °C |
326 ksi <br>@Strain 2.40 %,<br> Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 2.85 GPa <br>@Strain 1.10 %,<br> Temperature 23.0 °C |
413 ksi <br>@Strain 1.10 %,<br> Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 3.55 GPa <br>@Strain 1.70 %,<br> Temperature -40.0 °C |
515 ksi <br>@Strain 1.70 %,<br> Temperature -40.0 °F |
ISO 11403-1 -2 | |
| Izod Impact, Notched (ISO) | 11.0 kJ/m² | 5.23 ft-lb/in² | ISO 180/1A |
| 10.0 kJ/m² <br>@Temperature -40.0 °C |
4.76 ft-lb/in² <br>@Temperature -40.0 °F |
ISO 180/1A | |
| Charpy Impact, Notched | 1.20 J/cm² | 5.71 ft-lb/in² | ISO 179/1eA |
| 1.05 J/cm² <br>@Temperature -30.0 °C |
5.00 ft-lb/in² <br>@Temperature -22.0 °F |
ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 110 µm/m-°C | 61.1 µin/in-°F | ISO 11359-1/-2 |
| 100 µm/m-°C <br>@Temperature -40.0 - 23.0 °C |
55.6 µin/in-°F <br>@Temperature -40.0 - 73.4 °F |
ISO 11359-1/-2 | |
| CTE, linear, Transverse to Flow | 110 µm/m-°C | 61.1 µin/in-°F | ISO 11359-1/-2 |
| 100 µm/m-°C <br>@Temperature -40.0 - 23.0 °C |
55.6 µin/in-°F <br>@Temperature -40.0 - 73.4 °F |
ISO 11359-1/-2 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | IEC 60093 |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | IEC 60093 |
| Dielectric Constant | 3.9 <br>@Frequency 1.00e+6 Hz |
3.9 <br>@Frequency 1.00e+6 Hz |
IEC 60250 |
| 4.0 <br>@Frequency 100 Hz |
4.0 <br>@Frequency 100 Hz |
IEC 60250 | |
| Dielectric Strength | 45.0 kV/mm | 1140 kV/in | IEC 60243-1 |
| Dissipation Factor | 0.00050 <br>@Frequency 100 Hz |
0.00050 <br>@Frequency 100 Hz |
IEC 60250 |
| 0.0060 <br>@Frequency 1.00e+6 Hz |
0.0060 <br>@Frequency 1.00e+6 Hz |
IEC 60250 | |
| Comparative Tracking Index | 600 V | 600 V | IEC 60112 |