Category | Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate, Molded |
Manufacturer | Covestro |
Trade Name | Makrolon® |
Port | Shanghai port,China |
Trade Terms | FOB, CFR, CIF |
Payment Terms | L/C, T/T, Western Union |
Download PDF | Covestro Makrolon® 2400 Polycarbonate.pdf ![]() |
Price | EMAIL US sales@lookpolymers.com |
Physical Properties | Metric | English | Comments |
---|---|---|---|
Bulk Density | 0.660 g/cc | 0.0238 lb/in³ | pellets; ISO 60 |
Density | 1.20 g/cc | 0.0434 lb/in³ | ISO 1183-1 |
Moisture Absorption at Equilibrium | 0.12 % | 0.12 % | ISO 62, 50% RH |
Water Absorption at Saturation | 0.30 % | 0.30 % | ISO 62 |
Water Vapor Transmission | 15.0 g/m²/day @Thickness 0.100 mm |
0.966 g/100 in²/day @Thickness 0.00394 in |
85% RH, film; ISO 15106-1 |
Oxygen Transmission | 80.0 cc-mm/m²-24hr-atm @Thickness 0.0254 mm |
203 cc-mil/100 in²-24hr-atm @Thickness 0.00100 in |
3150 cc/m²-24hr-bar; film; b.o. ISO 2556 |
80.0 cc-mm/m²-24hr-atm @Thickness 0.100 mm |
203 cc-mil/100 in²-24hr-atm @Thickness 0.00394 in |
800 cc/m²-24hr-bar; film; b.o. ISO 2556 | |
Nitrogen Transmission | 16.0 cc-mm/m²-24hr-atm @Thickness 0.100 mm |
40.6 cc-mil/100 in²-24hr-atm @Thickness 0.00394 in |
160 cc/m²-24hr-bar; film; b.o. ISO 2556 |
16.0 cc-mm/m²-24hr-atm @Thickness 0.0254 mm |
40.6 cc-mil/100 in²-24hr-atm @Thickness 0.00100 in |
630 cc/m²-24hr-bar; film; b.o. ISO 2556 | |
Carbon Dioxide Transmission | 480 cc-mm/m²-24hr-atm @Thickness 0.0254 mm |
1220 cc-mil/100 in²-24hr-atm @Thickness 0.00100 in |
18900 cc/m²-24hr-bar; film; b.o. ISO 2556 |
480 cc-mm/m²-24hr-atm @Thickness 0.100 mm |
1220 cc-mil/100 in²-24hr-atm @Thickness 0.00394 in |
4800 cc/m²-24hr-bar; film; b.o. ISO 2556 | |
Linear Mold Shrinkage, Flow | 0.0065 cm/cm @Thickness 2.00 mm |
0.0065 in/in @Thickness 0.0787 in |
60x60x2 mm; 500 bar; ISO 294-4 |
Linear Mold Shrinkage, Transverse | 0.0065 cm/cm @Thickness 2.00 mm |
0.0065 in/in @Thickness 0.0787 in |
60x60x2 mm; 500 bar; ISO 294-4 |
Melt Flow | 20 g/10 min @Load 1.20 kg, Temperature 300 °C |
20 g/10 min @Load 2.65 lb, Temperature 572 °F |
ISO 1133 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Puncture Resistance | 5100 N @Temperature 23.0 °C |
1150 lb (f) @Temperature 73.4 °F |
ISO 6603-2 |
6000 N @Temperature -30.0 °C |
1350 lb (f) @Temperature -22.0 °F |
ISO 6603-2 | |
Ball Indentation Hardness | 113 MPa | 16400 psi | ISO 2039-1 |
Tensile Strength at Break | 70.0 MPa | 10200 psi | 50 mm/min; ISO 527-1,-2 |
Tensile Strength, Yield | 65.0 MPa | 9430 psi | 50 mm/min; ISO 527-1,-2 |
Elongation at Break | >= 50 % | >= 50 % | Nominal, 50 mm/min; ISO 527-1,-2 |
120 % | 120 % | 50 mm/min; b.o. ISO 527-1,-2 | |
Elongation at Yield | 6.3 % | 6.3 % | 50 mm/min; ISO 527-1,-2 |
Tensile Modulus | 2.35 GPa | 341 ksi | 1 mm/min; ISO 527-1,-2 |
Flexural Strength | 96.0 MPa | 13900 psi | 2 mm/min; ISO 178 |
Flexural Yield Strength | 72.0 MPa @Strain 3.50 % |
10400 psi @Strain 3.50 % |
2 mm/min; ISO 178 |
Flexural Modulus | 2.35 GPa | 341 ksi | 2 mm/min; ISO 178 |
Izod Impact, Notched (ISO) | 12.0 kJ/m² @Thickness 3.20 mm, Temperature -30.0 °C |
5.71 ft-lb/in² @Thickness 0.126 in, Temperature -22.0 °F |
complete break; b.o. ISO 180-A |
75.0 kJ/m² @Thickness 3.20 mm, Temperature 23.0 °C |
35.7 ft-lb/in² @Thickness 0.126 in, Temperature 73.4 °F |
partial break; b.o. ISO 180-A | |
Charpy Impact Unnotched | NB @Temperature 23.0 °C |
NB @Temperature 73.4 °F |
ISO 179-1eU |
NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
ISO 179-1eU | |
NB @Temperature -60.0 °C |
NB @Temperature -76.0 °F |
ISO 179-1eU | |
Charpy Impact, Notched | 1.40 J/cm² @Thickness 3.00 mm, Temperature -30.0 °C |
6.66 ft-lb/in² @Thickness 0.118 in, Temperature -22.0 °F |
complete break; ISO 7391/b.o. ISO 179-1eA |
6.50 J/cm² @Thickness 3.00 mm, Temperature 23.0 °C |
30.9 ft-lb/in² @Thickness 0.118 in, Temperature 73.4 °F |
partial break; ISO 7391/b.o. ISO 179-1eA | |
Puncture Energy | 55.0 J @Temperature 23.0 °C |
40.6 ft-lb @Temperature 73.4 °F |
ISO 6603-2 |
65.0 J @Temperature -30.0 °C |
47.9 ft-lb @Temperature -22.0 °F |
ISO 6603-2 | |
Tensile Creep Modulus, 1 hour | 2200 MPa | 319000 psi | ISO 899-1 |
Tensile Creep Modulus, 1000 hours | 1900 MPa | 276000 psi | ISO 899-1 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 65.0 µm/m-°C @Temperature 23.0 - 55.0 °C |
36.1 µin/in-°F @Temperature 73.4 - 131 °F |
ISO 11359-1,-2 |
CTE, linear, Transverse to Flow | 65.0 µm/m-°C @Temperature 23.0 - 55.0 °C |
36.1 µin/in-°F @Temperature 73.4 - 131 °F |
ISO 11359-1,-2 |
Thermal Conductivity | 0.200 W/m-K | 1.39 BTU-in/hr-ft²-°F | cross-flow; ISO 8302 |
Deflection Temperature at 0.46 MPa (66 psi) | 139 °C | 282 °F | ISO 75-1,-2 |
Deflection Temperature at 1.8 MPa (264 psi) | 127 °C | 261 °F | ISO 75-1,-2 |
Vicat Softening Point | 147 °C @Load 5.10 kg |
297 °F @Load 11.2 lb |
50°C/h; ISO 306 |
148 °C @Load 5.10 kg |
298 °F @Load 11.2 lb |
120°C/h; ISO 306 | |
Glass Transition Temp, Tg | 147 °C | 297 °F | 10°C/min; ISO 11357-1,-2 |
UL RTI, Electrical | 125 °C | 257 °F | UL 746B |
UL RTI, Mechanical with Impact | 115 °C | 239 °F | UL 746B |
UL RTI, Mechanical without Impact | 125 °C | 257 °F | UL 746B |
Flammability, UL94 | HB @Thickness 2.70 mm |
HB @Thickness 0.106 in |
|
V-2 @Thickness 0.750 mm |
V-2 @Thickness 0.0295 in |
||
Flash Point | 480 °C | 896 °F | ASTM D 1929 |
550 °C | 1020 °F | self ignition; ASTM D 1929 | |
Oxygen Index | 27 % | 27 % | Method A; ISO 4589-2 |
Glow Wire Test | 850 °C @Thickness 1.00 mm |
1560 °F @Thickness 0.0394 in |
GWFI; IEC 60695-2-12 |
850 °C @Thickness 1.50 mm |
1560 °F @Thickness 0.0591 in |
GWFI; IEC 60695-2-12 | |
850 °C @Thickness 2.00 mm |
1560 °F @Thickness 0.0787 in |
GWFI; IEC 60695-2-12 | |
875 °C @Thickness 1.00 mm |
1610 °F @Thickness 0.0394 in |
GWIT; IEC 60695-2-13 | |
875 °C @Thickness 1.50 mm |
1610 °F @Thickness 0.0591 in |
GWIT; IEC 60695-2-13 | |
875 °C @Thickness 2.00 mm |
1610 °F @Thickness 0.0787 in |
GWIT; IEC 60695-2-13 | |
875 °C @Thickness 3.00 mm |
1610 °F @Thickness 0.118 in |
GWIT; IEC 60695-2-13 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 1.00e+16 ohm-cm | 1.00e+16 ohm-cm | IEC 60093 |
Surface Resistance | 1.00e+16 ohm | 1.00e+16 ohm | IEC 60093 |
Dielectric Constant | 3.0 @Frequency 1.00e+6 Hz |
3.0 @Frequency 1.00e+6 Hz |
IEC 60250 |
3.1 @Frequency 100 Hz |
3.1 @Frequency 100 Hz |
IEC 60250 | |
Dielectric Strength | 34.0 kV/mm @Thickness 1.00 mm |
864 kV/in @Thickness 0.0394 in |
IEC 60243-1 |
Dissipation Factor | 0.00050 @Frequency 100 Hz |
0.00050 @Frequency 100 Hz |
IEC 60250 |
0.0090 @Frequency 1.00e+6 Hz |
0.0090 @Frequency 1.00e+6 Hz |
IEC 60250 | |
Comparative Tracking Index | 125 V | 125 V | CTI M; Solution B; IEC 60112 |
250 V | 250 V | Solution A; IEC 60112 |