Physical Properties | Metric | English | Comments |
---|---|---|---|
Linear Mold Shrinkage, Transverse | 0.0040 - 0.0075 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0075 in/in @Thickness 0.126 in |
SABIC Method |
SABIC Innovative Plastics Geloy XTWM206 ASA Next generation ASA optimized for outstanding weatherability, colorability and higher heat applications requiring UV exposure resistance.This data was supplied by SABIC-IP for the Americas region. |
|||
Linear Mold Shrinkage, Transverse | 0.0040 - 0.0075 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0075 in/in @Thickness 0.126 in |
SABIC Method |
SABIC Innovative Plastics Geloy XTWM206 ASA (Asia Pacific) Next generation ASA optimized for outstanding weatherability, colorability and higher heat applications requiring UV exposure resistance.This data was supplied by SABIC-IP for the Asia Pacific regio.. |
|||
Linear Mold Shrinkage, Transverse | 0.0040 - 0.0075 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0075 in/in @Thickness 0.126 in |
SABIC Method |
SABIC Innovative Plastics Geloy XTWM206 ASA (Europe-Africa-Middle East) Next generation ASA optimized for outstanding weatherability, colorability and higher heat applications requiring UV exposure resistance.This data was supplied by SABIC-IP for the Europe-Africa-Midd.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Lastilac 10 ABS/PC ABS/PC Blend (ABS/PC). Unfilled. Very good surface appearance. High impact resistance. Good thermal properties.Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaI.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Latamid 6 H2E04 G/30 PA 6, 30% Glass Fiber Reinforced, Heat Stabilized Polyamide 6 (PA6) based compound. Heat stabilized. Toughened. Glass fibers. Good elongation.Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Laril 13 G/10-V1 PPOm, 10% Glass Fiber Reinforced, Flame Retardant Modified Polyphenylene Oxide (PPOm) based compound. Glass fibers. UL94 V-1 classified, with brominated flame retardants, PBB/PBDE and antimony trioxide free. Very high dimensional stability. Good th.. |
|||
Linear Mold Shrinkage, Transverse | 0.0050 - 0.0075 cm/cm | 0.0050 - 0.0075 in/in | |
LATI Larpeek 10 G/40 PEEK, 40% Glass Fiber Reinforced Polyetheretherketone (PEEK) based compound. Glass fibers. Very good chemical resistance. Very good thermal properties. Low smoke density and low toxicity index.Availability: Africa & Middle East; As.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Latamid 6 H2 G/30-V0AF PA 6, 30% Glass Fiber Reinforced, Heat Stabilized, Flame Retardant Polyamide 6 (PA6) based compound. Heat stabilized. Glass fibers. UL94 V-0 classified, with brominated flame retardants, PBB/PBDE and antimony trioxide free. Availability: Africa & Middle East; Asia .. |
|||
Linear Mold Shrinkage, Transverse | 0.0050 - 0.0075 cm/cm | 0.0050 - 0.0075 in/in | |
LATI Laticonther 87/28 GR/50 PC, 50% Graphite Reinforced High thermal conductivity product based on Polycarbonate (PC). Graphite.Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided by Lati Industria T.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilon 28D-V0 PC, Flame Retardant Polycarbonate (PC) based compound. UL94 V-0 classified, brominated and chlorinated halogens-based flame retardants free. Low smoke density and low toxicity index. Very high dimensional stability. Ve.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilon 30D G/10-V0 PC, 10% Glass Fiber Reinforced, Flame Retardant Polycarbonate (PC) based compound. Glass fibers. UL94 V-0 classified, brominated and chlorinated halogens-based flame retardants free. Low smoke density and low toxicity index. High dimensional stab.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilub 87/24UV-20T PC, PTFE Filled Self-lubricating product based on Polycarbonate (PC). UV stabilized. PTFE. Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided by Lati Industri.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilub 87/28-20T PC, PTFE Filled Self-lubricating product based on Polycarbonate (PC). PTFE.Information provided by Lati Industria Termoplastici S.p.A. |
|||
Linear Mold Shrinkage, Transverse | 0.0050 - 0.0075 cm/cm | 0.0050 - 0.0075 in/in | |
LATI Latiohm 87/26-06 PD01-V1 PC, Flame Retardant Semiconductive/dissipative product based on Polycarbonate (PC). UL94 V-1 classified, with brominated flame retardants, PBB/PBDE and antimony trioxide free. Availability: Africa & Middle East; Asia .. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latiohm 87/28-07 CNT PC Semiconductive/dissipative product based on Polycarbonate (PC). Carbon nanotubes. Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided by Lati I.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Latishield 36/AR-08A G/17-V0E ABS, Steel/Glass Fiber Reinforced, Flame Retardant EMI shielding product based on Acrylonitrile-Butadiene-Styrene copolymer (ABS). Steel fibers. Glass fibers. UL94 V-0 classified, with brominated flame retardants, PBB/PBDE free. Availability: Africa.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latishield 87/28-10A PC, Steel Fiber Reinforced EMI shielding product based on Polycarbonate (PC). Steel fibers.Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided by Lati Industria Termoplas.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm @Thickness 3.20 mm |
0.0055 - 0.0075 in/in @Thickness 0.126 in |
SABIC Method |
SABIC Innovative Plastics NORYL BN9003G PPE+HIPS PPE+PS blend. Unfilled. Blow molding. Excellent balance of impact and surface aesthetics. Suitable for automotive exterior components including spoilers. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm @Thickness 3.00 mm |
0.0055 - 0.0075 in/in @Thickness 0.118 in |
150x105x3mm; b.o. ISO 2577 |
Covestro Bayblend® M850 XF PC/ABS Blend Main characteristics:• High toughness even at low temperatures• High dimensional accuracy and stability• Good paintability• Good flowabilityGrade characteristics:• Injection molding• Eas.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm @Thickness 3.00 mm |
0.0055 - 0.0075 in/in @Thickness 0.118 in |
150x105x3mm; b.o. ISO 2577 |
Covestro Bayblend® T50 BBS083 PC/ABS Blend Main characteristics:• High toughness even at low temperatures• High dimensional accuracy and stability• Good paintability• Good flowabilityGrade characteristics:• Injection molding• Goo.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm @Thickness 3.00 mm |
0.0055 - 0.0075 in/in @Thickness 0.118 in |
150x105x3mm; b.o. ISO 2577 |
Covestro Bayblend® T80 XG PC/ABS Blend Main characteristics:• High toughness even at low temperatures• High dimensional accuracy and stability• Good paintability• Good flowabilityGrade characteristics:• Injection molding• Opt.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm @Thickness 3.00 mm |
0.0055 - 0.0075 in/in @Thickness 0.118 in |
150x105x3mm; b.o. ISO 2577 |
Covestro Bayblend® T85 SG PC/ABS Blend Main characteristics:• High toughness even at low temperatures• High dimensional accuracy and stability• Good paintability• Good flowabilityGrade characteristics:• Injection molding• Hig.. |
|||
Linear Mold Shrinkage, Transverse | 0.0055 - 0.0075 cm/cm | 0.0055 - 0.0075 in/in | |
LATI Kelon® A FR H2 CETG/300-V0 PA 66, Glass/Mineral Reinforced, Flame Retardant, Heat Stabilized Polyamide 66 (PA66) based compound. Heat stabilized. Glass fibers / Mineral filler. UL94 V-0 classified, with brominated flame retardants, PBB/PBDE and antimony trioxide free. Low thermal expansion .. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Lapex A G/30 PES, 30% Glass Fiber Reinforced Polyether Sulfone (PES) based compound. Glass fibers. Low smoke density and low toxicity index. Very high dimensional stability.Availability: Africa & Middle East; Asia Pacific; Europe; Latin Americ.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilon 30D-V0 PC, Flame Retardant Polycarbonate (PC) based compound. UL94 V-0 classified, brominated and chlorinated halogens-based flame retardants free. Low smoke density and low toxicity index. Very high dimensional stability. Ve.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilub 80-15T G/30 PPS, 30% Glass Fiber Reinforced, PTFE Filled Self-lubricating product based on Polyphenylene Sulfide (PPS). PTFE. Glass fibers.Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provided by Lati I.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Latilub 80-17ST G/30 PPS, 30% Glass Fiber Reinforced, Silicone/PTFE Filled Self-lubricating product based on Polyphenylene Sulfide (PPS). Silicone / PTFE. Glass fibers. Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North AmericaInformation provid.. |
|||
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0075 cm/cm | 0.0060 - 0.0075 in/in | |
LATI Kelon® A FR H2 CET/35-V2 PA 66, 35% Mineral Reinforced, Flame Retardant, Heat Stabilized Polyamide 66 (PA66) based compound. Heat stabilized. Mineral filler. UL94 V-2 classified, with brominated flame retardants, PBB/PBDE free.Availability: Africa & Middle East; Asia Pacific; Europe; La.. |