Solvay Specialty Polymers Amodel® AS-4133 HN Polyphthalamide (PPA), Dry, 33% Glass Fiber Reinforcement, Heat Stabilizer

Category Polymer , Thermoplastic , Polyphthalamide (PPA) , Polyphthalamide (PPA), 30% Glass Fiber Reinforced
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers Amodel® AS-4133 HN Polyphthalamide (PPA), Dry, 33% Glass Fiber Reinforcement, Heat Stabilizer.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Amodel AS-4133 HN polyphthalamide (PPA) is a non-lubricated, heat stabilized grade that offers fast cycle times and is hot-water moldable. Typical applications include electrical and electronic components especially for automotive systems.- Black: AS-4133 HN BK 543Features: Fast Molding Cycle; Good Chemical Resistance; Good Creep Resistance; Good Dimensional Stability; Good Stiffness; Heat Stabilized; High Heat Resistance; High Strength; Hot Water Moldability; Low Moisture AbsorptionUses: Automotive Applications; Automotive Under the Hood; Connectors; General Purpose; Industrial Applications; Lawn and Garden Equipment; Machine/Mechanical Parts; Metal Replacement; Valves/Valve PartsAvailability: Africa & Middle East; Asia Pacific; Europe; North America; South AmericaInjection Rate: 3 to 4 in/secHolding Pressure: 50% of injection pressureInformation provide by Solvay Specialty Polymers
Physical Properties Metric English Comments
Density 1.45 g/cc
0.0524 lb/in³
ISO 1183 Method A
Water Absorption 0.29 %
0.29 %
24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0050 cm/cm
0.0050 in/in
ASTM D955
Linear Mold Shrinkage, Transverse 0.010 cm/cm
0.010 in/in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 79.3 MPa

@Temperature 175 °C
11500 psi

@Temperature 347 °F
ISO 527-2
87.6 MPa

@Temperature 150 °C
12700 psi

@Temperature 302 °F
ISO 527-2
125 MPa

@Temperature 100 °C
18100 psi

@Temperature 212 °F
ISO 527-2
211 MPa

@Temperature 23.0 °C
30600 psi

@Temperature 73.4 °F
ISO 527-2
Tensile Strength 200 MPa
29000 psi
ASTM D638
Elongation at Break 2.5 %
2.5 %
ASTM D638
2.6 %

@Temperature 23.0 °C
2.6 %

@Temperature 73.4 °F
ISO 527-2
4.3 %

@Temperature 100 °C
4.3 %

@Temperature 212 °F
ISO 527-2
6.6 %

@Temperature 175 °C
6.6 %

@Temperature 347 °F
ISO 527-2
6.6 %

@Temperature 150 °C
6.6 %

@Temperature 302 °F
ISO 527-2
Tensile Modulus 11.7 GPa
1700 ksi
ASTM D638
4.83 GPa

@Temperature 175 °C
701 ksi

@Temperature 347 °F
ISO 527-2
5.31 GPa

@Temperature 150 °C
770 ksi

@Temperature 302 °F
ISO 527-2
6.83 GPa

@Temperature 100 °C
991 ksi

@Temperature 212 °F
ISO 527-2
12.6 GPa

@Temperature 23.0 °C
1830 ksi

@Temperature 73.4 °F
ISO 527-2
Flexural Strength 290 MPa
42100 psi
ASTM D790
99.3 MPa

@Temperature 175 °C
14400 psi

@Temperature 347 °F
ISO 178
111 MPa

@Temperature 150 °C
16100 psi

@Temperature 302 °F
ISO 178
177 MPa

@Temperature 100 °C
25700 psi

@Temperature 212 °F
ISO 178
296 MPa

@Temperature 23.0 °C
42900 psi

@Temperature 73.4 °F
ISO 178
Flexural Modulus 11.0 GPa
1600 ksi
ASTM D790
4.21 GPa

@Temperature 175 °C
611 ksi

@Temperature 347 °F
ISO 178
4.62 GPa

@Temperature 150 °C
670 ksi

@Temperature 302 °F
ISO 178
7.17 GPa

@Temperature 100 °C
1040 ksi

@Temperature 212 °F
ISO 178
10.4 GPa

@Temperature 23.0 °C
1510 ksi

@Temperature 73.4 °F
ISO 178
Compressive Strength 179 MPa
26000 psi
ASTM D695
Poissons Ratio 0.41
0.41
ASTM E132
Shear Modulus 4.15 - 4.47 GPa
602 - 648 ksi
Calculated
Shear Strength 89.6 MPa
13000 psi
ASTM D732
Izod Impact, Notched 0.800 J/cm
1.50 ft-lb/in
ASTM D256
Izod Impact, Unnotched 9.60 J/cm
18.0 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 9.70 kJ/m²
4.62 ft-lb/in²
23°C, Type 1, Notch A; ISO 180
Izod Impact, Unnotched (ISO) 59.0 kJ/m²
28.1 ft-lb/in²
23°C, Type 1; ISO 180
Charpy Impact Unnotched 6.70 J/cm²
31.9 ft-lb/in²
23°C, Type 1, Edgewise; ISO 179
Charpy Impact, Notched 1.10 J/cm²
5.23 ft-lb/in²
23°C, Type 1, Edgewise, Notch A; ISO 179
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 14.0 µm/m-°C

@Temperature 149 - 249 °C
7.78 µin/in-°F

@Temperature 300 - 480 °F
ASTM E831
22.0 µm/m-°C

@Temperature 0.000 - 90.0 °C
12.2 µin/in-°F

@Temperature 32.0 - 194 °F
ASTM E831
CTE, linear, Transverse to Flow 59.0 µm/m-°C

@Temperature 0.000 - 90.0 °C
32.8 µin/in-°F

@Temperature 32.0 - 194 °F
ASTM E831
120 µm/m-°C

@Temperature 149 - 249 °C
66.7 µin/in-°F

@Temperature 300 - 480 °F
ASTM E831
Melting Point 327 °C
621 °F
ISO 11357-3
327 °C
621 °F
Maximum Service Temperature, Air 210 °C
410 °F
ASTM D794
Deflection Temperature at 0.46 MPa (66 psi) 320 °C

@Thickness 3.20 mm
608 °F

@Thickness 0.126 in
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 294 °C
561 °F
Unannealed; ISO 75-2/A
300 °C

@Thickness 3.20 mm
572 °F

@Thickness 0.126 in
Annealed; ASTM D648
Flammability, UL94 HB

@Thickness 3.20 mm
HB

@Thickness 0.126 in
Electrical Properties Metric English Comments
Volume Resistivity 2.00e+16 ohm-cm
2.00e+16 ohm-cm
ASTM D257
Dielectric Constant 3.6

@Frequency 1.00e+6 Hz
3.6

@Frequency 1.00e+6 Hz
ASTM D150
3.8

@Frequency 60.0 Hz
3.8

@Frequency 60.0 Hz
ASTM D150
Dielectric Strength 20.0 kV/mm

@Thickness 1.60 mm
508 kV/in

@Thickness 0.0630 in
ASTM D149
Dissipation Factor 0.0040

@Frequency 60.0 Hz
0.0040

@Frequency 60.0 Hz
ASTM D150
0.012

@Frequency 1.00e+6 Hz
0.012

@Frequency 1.00e+6 Hz
ASTM D150
Comparative Tracking Index 600 V
600 V
High Voltage Arc-Tracking Rate, HVTR 14.0 mm/min
0.551 in/min
UL 746
Processing Properties Metric English Comments
Rear Barrel Temperature 318 - 324 °C
604 - 615 °F
Front Barrel Temperature 327 - 332 °C
621 - 630 °F
Melt Temperature 329 - 343 °C
624 - 649 °F
Mold Temperature 65.6 - 93.3 °C
150 - 200 °F
Drying Temperature 120 °C
248 °F
Dry Time 4 hour
4 hour
Moisture Content 0.045 %
0.045 %
suggested max
Descriptive Properties Value Comments
Appearance Black
Automotive Specifications ASTM D4000 PA102 G35 Color: BK324 Black
ASTM D4000 PA102 G35 Color: NT Natural
ASTM D4000 PPA0121 G34 GB145 KD170 KN100 PN060 YI285 Color: BK324 Black
ASTM D4000 PPA0121 G34 GB145 KD170 KN100 PN060 YI285 Color: NT Natural
BOSCH N28 BN05-OX2 Color: BK324 Black
BOSCH N28 BN05-OX2 Color: NT Natural
CHRYSLER MS-DB478 Type A CPN3598 Color: BK Black
CHRYSLER MS-DB478 Type A CPN3972 Color: Natural
DELPHI M-2396 Color: BK
DELPHI M-2396 Color: BK324 Black
DELPHI M-2396 Color: BU474 Blue
DELPHI M-2396 Color: NT Natural
DELPHI M-53291 Color: BU474 Blue
DELPHI M-53293 Color: BK324 Black
DELPHI M-53293 Color: NT Natural