| Category | Polymer , Thermoplastic , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | LNP LUBRICOMP |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | SABIC Innovative Plastics LNP LUBRICOMP DFL329 PC.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.40 g/cc | 0.0506 lb/in³ | ISO 1183 |
| 1.40 g/cc | 0.0506 lb/in³ | ASTM D792 | |
| Moisture Absorption | 0.120 % | 0.120 % | 50% RH, 24 hrs; ASTM D570 |
| 0.150 % | 0.150 % | 23°C / 50% RH; ISO 62 | |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm @Time 86400 sec |
0.0030 in/in @Time 24.0 hour |
ASTM D955 |
| 0.0033 cm/cm @Time 86400 sec |
0.0033 in/in @Time 24.0 hour |
ISO 294 | |
| Linear Mold Shrinkage, Transverse | 0.0049 cm/cm @Time 86400 sec |
0.0049 in/in @Time 24.0 hour |
ISO 294 |
| 0.0050 cm/cm @Time 86400 sec |
0.0050 in/in @Time 24.0 hour |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 74.0 MPa | 10700 psi | ISO 527 |
| 75.0 MPa | 10900 psi | ASTM D638 | |
| Elongation at Break | 3.0 % | 3.0 % | ISO 527 |
| 3.0 % | 3.0 % | ASTM D638 | |
| Tensile Modulus | 4.34 GPa | 629 ksi | 50 mm/min; ASTM D638 |
| 4.50 GPa | 653 ksi | 1 mm/min; ISO 527 | |
| Flexural Strength | 127 MPa | 18400 psi | ISO 178 |
| 129 MPa | 18700 psi | ASTM D790 | |
| Flexural Modulus | 4.27 GPa | 619 ksi | ASTM D790 |
| 4.60 GPa | 667 ksi | ISO 178 | |
| Izod Impact, Notched | 1.81 J/cm | 3.39 ft-lb/in | ASTM D256 |
| Izod Impact, Unnotched | 5.50 J/cm | 10.3 ft-lb/in | ASTM D4812 |
| Izod Impact, Notched (ISO) | 9.00 kJ/m² | 4.28 ft-lb/in² | 80*10*4; ISO 180/1A |
| Izod Impact, Unnotched (ISO) | 38.0 kJ/m² | 18.1 ft-lb/in² | 80*10*4; ISO 180/1U |
| Dart Drop, Total Energy | 18.0 J | 13.3 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
| Impact Test | 3.00 J | 2.21 ft-lb | Multiaxial Impact; ISO 6603 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 44.8 µm/m-°C @Temperature -40.0 - 40.0 °C |
24.9 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 |
| 44.8 µm/m-°C @Temperature -40.0 - 40.0 °C |
24.9 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 | |
| CTE, linear, Transverse to Flow | 49.8 µm/m-°C @Temperature -40.0 - 40.0 °C |
27.7 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 49.9 µm/m-°C @Temperature -40.0 - 40.0 °C |
27.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Deflection Temperature at 0.46 MPa (66 psi) | 146 °C @Thickness 3.20 mm |
295 °F @Thickness 0.126 in |
unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 141 °C | 286 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 141 °C @Thickness 3.20 mm |
286 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Flammability, UL94 | V-0 @Thickness 1.70 mm |
V-0 @Thickness 0.0669 in |
UL 94 by SABIC-IP |