| Category | Polymer , Thermoplastic , Fluoropolymer , ETFE/ECTFE , ECTFE Fluoropolymer |
| Manufacturer | Isoflon |
| Trade Name | |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Isoflon ECTFE Fluoropolymer.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.67 - 1.70 g/cc | 1.67 - 1.70 g/cc | ISO 12086 |
| Water Absorption | 0.010 % | 0.010 % | DIN 53 495 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 70 - 80 | 70 - 80 | DIN 53 505 |
| Ball Indentation Hardness | 55.0 - 65.0 MPa | 7980 - 9430 psi | DIN 53 456 |
| Tensile Strength | 40.0 - 55.0 MPa | 5800 - 7980 psi | DIN 53455 |
| Elongation at Break | 200 - 300 % | 200 - 300 % | DIN 53455 |
| Tensile Modulus | 1.20 - 1.80 GPa | 174 - 261 ksi | DIN 53457 |
| Coefficient of Friction, Dynamic | 0.65 | 0.65 | on steel |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 80.0 µm/m-°C @Temperature 20.0 - 100 °C |
44.4 µin/in-°F @Temperature 68.0 - 212 °F |
|
| Thermal Conductivity | 0.150 W/m-K | 1.04 BTU-in/hr-ft²-°F | DIN 52612 |
| Maximum Service Temperature, Air | 150 °C | 302 °F | Continuous |
| Minimum Service Temperature, Air | -75.0 °C | -103 °F | Continuous |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Dielectric Strength | 50.0 - 80.0 kV/mm | 1270 - 2030 kV/in | DIN 53481 |