| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.46 g/cc | 0.0527 lb/in³ | DAM; ISO 1183 |
| Filler Content | 30 % | 30 % | DAM |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm @Thickness 2.00 mm |
0.0030 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.010 cm/cm @Thickness 2.00 mm |
0.010 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 135 MPa @Temperature 23.0 °C |
19600 psi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 145 MPa @Temperature 23.0 °C |
21000 psi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Elongation at Break | 1.9 % @Temperature 23.0 °C |
1.9 % @Temperature 73.4 °F |
50%RH; ISO 527 |
| 2.1 % @Temperature 23.0 °C |
2.1 % @Temperature 73.4 °F |
DAM; ISO 527 | |
| Tensile Modulus | 10.7 GPa @Temperature 23.0 °C |
1550 ksi @Temperature 73.4 °F |
DAM; ISO 527 |
| 11.3 GPa @Temperature 23.0 °C |
1640 ksi @Temperature 73.4 °F |
50%RH; ISO 527 | |
| Flexural Strength | 200 MPa @Temperature 23.0 °C |
29000 psi @Temperature 73.4 °F |
50%RH; ISO 178 |
| 225 MPa @Temperature 23.0 °C |
32600 psi @Temperature 73.4 °F |
DAM; ISO 178 | |
| Flexural Modulus | 9.80 GPa @Temperature 23.0 °C |
1420 ksi @Temperature 73.4 °F |
DAM; ISO 178 |
| 10.8 GPa @Temperature 23.0 °C |
1570 ksi @Temperature 73.4 °F |
50%RH; ISO 178 | |
| Charpy Impact Unnotched | 3.50 J/cm² @Temperature -30.0 °C |
16.7 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU |
| 4.00 J/cm² @Temperature -30.0 °C |
19.0 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU | |
| 4.00 J/cm² @Temperature 23.0 °C |
19.0 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eU | |
| 4.50 J/cm² @Temperature 23.0 °C |
21.4 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eU | |
| Charpy Impact, Notched | 0.700 J/cm² @Temperature -30.0 °C |
3.33 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA |
| 0.700 J/cm² @Temperature -30.0 °C |
3.33 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA | |
| 0.700 J/cm² @Temperature 23.0 °C |
3.33 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eA | |
| 0.700 J/cm² @Temperature 23.0 °C |
3.33 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 500 µm/m-°C @Temperature -40.0 - 23.0 °C |
278 µin/in-°F @Temperature -40.0 - 73.4 °F |
DAM; ISO 11359-1/-2 |
| 500 µm/m-°C @Temperature 160 - 250 °C |
278 µin/in-°F @Temperature 320 - 482 °F |
DAM; ISO 11359-1/-2 | |
| 500 µm/m-°C @Temperature 23.0 - 55.0 °C |
278 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ISO 11359-1/-2 | |
| 500 µm/m-°C @Temperature 55.0 - 160 °C |
278 µin/in-°F @Temperature 131 - 320 °F |
DAM; ISO 11359-1/-2 | |
| CTE, linear, Transverse to Flow | 60.0 µm/m-°C @Temperature -40.0 - 23.0 °C |
33.3 µin/in-°F @Temperature -40.0 - 73.4 °F |
DAM; ISO 11359-1/-2 |
| 62.0 µm/m-°C @Temperature 23.0 - 55.0 °C |
34.4 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ISO 11359-1/-2 | |
| 95.0 µm/m-°C @Temperature 55.0 - 160 °C |
52.8 µin/in-°F @Temperature 131 - 320 °F |
DAM; ISO 11359-1/-2 | |
| 120 µm/m-°C @Temperature 160 - 250 °C |
66.7 µin/in-°F @Temperature 320 - 482 °F |
DAM; ISO 11359-1/-2 | |
| Melting Point | 310 °C | 590 °F | 10°C/min, First Heat; DAM; ISO 11357-1/-3 |
| Deflection Temperature at 1.8 MPa (264 psi) | 281 °C | 538 °F | DAM; ISO 75-1/-2 |
| UL RTI, Electrical | 140 °C @Thickness 0.750 mm |
284 °F @Thickness 0.0295 in |
DAM; UL 746B |
| 140 °C @Thickness 0.400 mm |
284 °F @Thickness 0.0157 in |
DAM; UL 746B | |
| 140 °C @Thickness 3.00 mm |
284 °F @Thickness 0.118 in |
DAM; UL 746B | |
| 140 °C @Thickness 1.50 mm |
284 °F @Thickness 0.0591 in |
DAM; UL 746B | |
| UL RTI, Mechanical with Impact | 115 °C @Thickness 0.750 mm |
239 °F @Thickness 0.0295 in |
DAM; UL 746B |
| 120 °C @Thickness 3.00 mm |
248 °F @Thickness 0.118 in |
DAM; UL 746B | |
| UL RTI, Mechanical without Impact | 125 °C @Thickness 0.750 mm |
257 °F @Thickness 0.0295 in |
DAM; UL 746B |
| 130 °C @Thickness 3.00 mm |
266 °F @Thickness 0.118 in |
DAM; UL 746B | |
| Flammability, UL94 | V-0 @Thickness 0.400 mm |
V-0 @Thickness 0.0157 in |
DAM; UL94 |
| V-0 @Thickness 3.00 mm |
V-0 @Thickness 0.118 in |
DAM; UL94 | |
| Glow Wire Test | 700 °C @Thickness 0.400 mm |
1290 °F @Thickness 0.0157 in |
DAM; Ignition; IEC 60695-2-13 |
| 775 °C @Thickness 3.00 mm |
1430 °F @Thickness 0.118 in |
DAM; Ignition; IEC 60695-2-13 | |
| 960 °C @Thickness 0.400 mm |
1760 °F @Thickness 0.0157 in |
DAM; IEC 60695-2-12 | |
| 960 °C @Thickness 3.00 mm |
1760 °F @Thickness 0.118 in |
DAM; IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Comparative Tracking Index | 600 V @Temperature 23.0 °C |
600 V @Temperature 73.4 °F |
DAM; IEC 60112 |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 320 - 325 °C | 608 - 617 °F | DAM |
| Mold Temperature | 85.0 - 130 °C | 185 - 266 °F | DAM |
| Drying Temperature | 100 °C | 212 °F | DAM |
| Dry Time | 6.00 - 8.00 hour | 6.00 - 8.00 hour | DAM |
| Moisture Content | <= 0.10 % | <= 0.10 % | DAM |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Appearance | Black Color | DAM |
| Filler | Glass Reinforced | DAM |
| Forms | Pellets | DAM |
| Generic | Polyphthalamide (PPA) | DAM |
| Material Status | Preliminary Data | DAM |
| Part Marking Code | >PA6T/66-GF30FR< | ISO 11469; DAM |
| >PPA-GF30FR< | SAE J1344; DAM | |
| Polymer Family | High performance polyamide | DAM |
| Polymer Type | Partially Aromatic PA, PPA | DAM |
| Processing Method | Injection Molding | DAM |
| Product Category | Flame Retardant Resins | DAM |
| Glass Reinforced Resins | DAM | |
| Region Available - Global | Yes | DAM |
| Resin Identification | PA6T/66-GF30FR | ISO 1043; DAM |
| RoHS Compliance | Contact Manufacturer | DAM |