| Category | Polymer , Thermoplastic , Nylon , Nylon 612 , Nylon 612, Glass Fiber Filler |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® FG77G33L NC010 Nylon 612.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.32 g/cc | 0.0477 lb/in³ | DAM; ISO 1183 |
| Water Absorption | 1.8 % @Thickness 2.00 mm |
1.8 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Moisture Absorption | 0.700 % @Thickness 2.00 mm |
0.700 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Water Absorption at Saturation | 0.30 % | 0.30 % | DAM; Immersion 24h; ASTM D570 |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm | 0.0030 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.0090 cm/cm | 0.0090 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 140 MPa | 20300 psi | 50%RH; ISO 527-1/-2 |
| 168 MPa | 24400 psi | DAM; ISO 527-1/-2 | |
| Elongation at Break | 3.2 % | 3.2 % | DAM; ISO 527-1/-2 |
| 3.2 % | 3.2 % | 50%RH; ISO 527-1/-2 | |
| Tensile Modulus | 7.90 GPa | 1150 ksi | 50%RH; ISO 527-1/-2 |
| 9.50 GPa | 1380 ksi | DAM; ISO 527-1/-2 | |
| Flexural Modulus | 7.00 GPa | 1020 ksi | 50%RH; ISO 178 |
| 8.20 GPa | 1190 ksi | DAM; ISO 178 | |
| Izod Impact, Notched (ISO) | 12.0 kJ/m² | 5.71 ft-lb/in² | 50%RH; ISO 180/1A |
| 13.0 kJ/m² | 6.19 ft-lb/in² | DAM; ISO 180/1A | |
| 10.0 kJ/m² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1A | |
| 10.0 kJ/m² @Temperature -40.0 °C |
4.76 ft-lb/in² @Temperature -40.0 °F |
50%RH; ISO 180/1A | |
| 11.0 kJ/m² @Temperature -40.0 °C |
5.23 ft-lb/in² @Temperature -40.0 °F |
DAM; ISO 180/1A | |
| 11.0 kJ/m² @Temperature -30.0 °C |
5.23 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1A | |
| Izod Impact, Unnotched (ISO) | 60.0 kJ/m² | 28.6 ft-lb/in² | 50%RH; ISO 180/1U |
| 70.0 kJ/m² | 33.3 ft-lb/in² | DAM; ISO 180/1U | |
| 45.0 kJ/m² @Temperature -30.0 °C |
21.4 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1U | |
| 60.0 kJ/m² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1U | |
| Charpy Impact Unnotched | 8.00 J/cm² | 38.1 ft-lb/in² | DAM; ISO 179/1eU |
| 9.00 J/cm² | 42.8 ft-lb/in² | 50%RH; ISO 179/1eU | |
| 6.00 J/cm² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU | |
| 6.50 J/cm² @Temperature -30.0 °C |
30.9 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU | |
| Charpy Impact, Notched | 1.20 J/cm² | 5.71 ft-lb/in² | 50%RH; ISO 179/1eA |
| 1.30 J/cm² | 6.19 ft-lb/in² | DAM; ISO 179/1eA | |
| 1.00 J/cm² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA | |
| 1.00 J/cm² @Temperature -40.0 °C |
4.76 ft-lb/in² @Temperature -40.0 °F |
50%RH; ISO 179/1eA | |
| 1.10 J/cm² @Temperature -30.0 °C |
5.23 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA | |
| 1.20 J/cm² @Temperature -40.0 °C |
5.71 ft-lb/in² @Temperature -40.0 °F |
DAM; ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 17.0 µm/m-°C | 9.44 µin/in-°F | DAM; ISO 11359-1/-2 |
| 16.0 µm/m-°C @Temperature 55.0 - 160 °C |
8.89 µin/in-°F @Temperature 131 - 320 °F |
DAM; ISO 11359-1/-2 | |
| 26.0 µm/m-°C @Temperature -40.0 - 23.0 °C |
14.4 µin/in-°F @Temperature -40.0 - 73.4 °F |
DAM; ISO 11359-1/-2 | |
| CTE, linear, Transverse to Flow | 113 µm/m-°C | 62.8 µin/in-°F | DAM; ISO 11359-1/-2 |
| 83.0 µm/m-°C @Temperature -40.0 - 23.0 °C |
46.1 µin/in-°F @Temperature -40.0 - 73.4 °F |
DAM; ISO 11359-1/-2 | |
| 158 µm/m-°C @Temperature 55.0 - 160 °C |
87.8 µin/in-°F @Temperature 131 - 320 °F |
DAM; ISO 11359-1/-2 | |
| Specific Heat Capacity | 2.13 J/g-°C | 0.509 BTU/lb-°F | |
| Thermal Conductivity | 0.260 W/m-K | 1.80 BTU-in/hr-ft²-°F | of melt |
| Melting Point | 218 °C | 424 °F | DAM; 10°C/min; ISO 11357-1/-3 |
| Deflection Temperature at 0.46 MPa (66 psi) | 216 °C | 421 °F | DAM; ISO 75-1/-2 |
| Deflection Temperature at 1.8 MPa (264 psi) | 200 °C | 392 °F | DAM; ISO 75-1/-2 |
| Glass Transition Temp, Tg | 65.0 °C | 149 °F | DAM; 10°C/min; ISO 11357-1/-2 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Additives | Release agent | |
| Delivery Form | Pellets | |
| Part Marking Code | >PA612-GF33< | ISO 11469 |
| Processing | Injection Moulding | |
| Regional Availability | Asia Pacific | |
| Europe | ||
| Global | ||
| Near East/Africa | ||
| North America | ||
| South and Central America | ||
| Resin Identification | PA612-GF33 | |