Category | Polymer , Thermoplastic , Polyphenylene Ether/PPO , Polyphenylene Ether, Heat Resistant |
Manufacturer | Asahi Kasei |
Trade Name | Xyron® |
Port | Shanghai port,China |
Trade Terms | FOB, CFR, CIF |
Payment Terms | L/C, T/T, Western Union |
Download PDF | Asahi Kasei Xyron® 140V Modified Polyphenylene Ether.pdf ![]() |
Price | EMAIL US sales@lookpolymers.com |
Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gravity | 1.08 g/cc | 1.08 g/cc | 23°C; ASTM D792 |
Moisture Absorption | 0.100 % | 0.100 % | 23°C, 50% RH 24 hours; ASTM D570 |
Linear Mold Shrinkage | 0.0050 - 0.0070 cm/cm | 0.0050 - 0.0070 in/in | ASTM D955 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Tensile Strength, Yield | 44.0 MPa | 6380 psi | 23°C, 50% RH; ASTM D638 |
Elongation at Break | 40 % | 40 % | 23°C, 50% RH; ASTM D638 |
Flexural Strength | 64.0 MPa | 9280 psi | 23°C, 50% RH; ASTM D790 |
Flexural Modulus | 2.30 GPa | 334 ksi | 23°C, 50% RH; ASTM D790 |
Izod Impact, Notched | 1.18 J/cm @Thickness 6.40 mm, Temperature 23.0 °C |
2.21 ft-lb/in @Thickness 0.252 in, Temperature 73.4 °F |
ASTM D256 |
1.76 J/cm @Thickness 3.20 mm, Temperature 23.0 °C |
3.30 ft-lb/in @Thickness 0.126 in, Temperature 73.4 °F |
ASTM D256 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear | 80.0 µm/m-°C @Temperature -30.0 - 60.0 °C |
44.4 µin/in-°F @Temperature -22.0 - 140 °F |
ASTM D696 |
Deflection Temperature at 1.8 MPa (264 psi) | 85.0 °C | 185 °F | ASTM D648 |
Flammability, UL94 | V-1 @Thickness 1.60 mm |
V-1 @Thickness 0.0630 in |
|
V-1 @Thickness 3.20 mm |
V-1 @Thickness 0.126 in |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 1.00e+16 ohm-cm | 1.00e+16 ohm-cm | 50% RH; ASTM D257 |
Surface Resistance | 1.00e+16 ohm | 1.00e+16 ohm | 50% RH; ASTM D257 |
Dielectric Constant | 2.9 @Frequency 1e+6 Hz |
2.9 @Frequency 1e+6 Hz |
50% RH; ASTM D150 |
2.9 @Frequency 1e+6 Hz |
2.9 @Frequency 1e+6 Hz |
50% RH; ASTM D150 | |
Dielectric Strength | 29.0 kV/mm @Thickness 2.00 mm |
737 kV/in @Thickness 0.0787 in |
Short time; ASTM D149 |
Dissipation Factor | 0.0030 @Frequency 60 Hz |
0.0030 @Frequency 60 Hz |
50% RH; ASTM D150 |
0.0040 @Frequency 1e+6 Hz |
0.0040 @Frequency 1e+6 Hz |
50% RH; ASTM D150 | |
Arc Resistance | 100 sec | 100 sec | Tungsten; ASTM D495 |
Processing Properties | Metric | English | Comments |
---|---|---|---|
Processing Temperature | 220 - 270 °C | 428 - 518 °F | Resin Temperature |
Mold Temperature | 40.0 - 70.0 °C | 104 - 158 °F | |
Drying Temperature | 70.0 - 80.0 °C | 158 - 176 °F | Pre-drying Temperature |
Dry Time | 2 - 4 hour | 2 - 4 hour |