Material Notes:
Termoton®V, TPV compounds with a dynamically cured EPDM phase closely dispersed in a polyolefin phase (PP). Main Characteristics: Wide range of hardness; High strength elasticity; 100% recyclable; Easy processing by means of the traditional technologies for thermoplastic materials; Additional resistance to heat, UV, O, and weathering; Excellent resistance to several chemical agents like bases, acids, alcohols, detergents etc; Transparency-easy coloring; Heat adhesion on rigid polymeric materials like PA, PC, ABS, PMMA, PS, SAN, TPU polymers; High elastic recovery within a wide temperature range; Soft rubbery touch, excellent wet and dry grip; Low compression set even at high temperature; High fatigue resistance; High thermal and electric insulation values; Good abrasion resistance; Many products meet FDA and REACH regulationsInformation provided by Termopol Termoplastik Elastomer
Physical Properties Metric English Comments
Density 0.960 g/cc
0.0347 lb/in³
ISO 2781
Mechanical Properties Metric English Comments
Hardness, Shore D 50
50
ISO 868
Tensile Strength 19.0 MPa
2760 psi
ISO 37
Elongation at Break 600 %
600 %
ISO 37
100% Modulus 0.00900 GPa
1.31 ksi
ISO 37
300% Modulus 0.00100 GPa
0.145 ksi
ISO 37
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 125 °C
257 °F
Minimum Service Temperature, Air -50.0 °C
-58.0 °F
Flammability, UL94 V-0
V-0
Processing Properties Metric English Comments
Drying Temperature 90.0 °C

@Time 7200 sec
194 °F

@Time 2.00 hour
Back Pressure 0.340 MPa
49.3 psi
Screw Speed 25 - 75 rpm
25 - 75 rpm
Descriptive Properties Value Comments
Acid-Base Resistance Excellent
Alcohol Resistance Excellent
Compression Set Very Good
Injection Pressure Medium
Injection Speed Medium-high
Motor Oil Resistance Good
Plasticizing Speed High
Solvent Resistance Good
UV-Ozone Stability Excellent
Users viewing this material also viewed the following: