Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 60 PHR Non-Black, Hi-Sil 233

Category Polymer , Thermoset , Polyester, TS , Polyurethane, TS , Thermoset Polyurethane, Elastomer, Unreinforced , Rubber or Thermoset Elastomer (TSE)
Manufacturer TSE Industries, Inc
Trade Name Millathane®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 60 PHR Non-Black, Hi-Sil 233.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Millathane® 76 is a very suitable choice for use in products such as bushings, small copier rolls; automotive applications — bumpers, o-rings, hydraulic seals, belts, gaskets, solid tires — and many other high performance polyurethane applications. Millathane 76 can be vulcanized by sulfur or peroxide cured systems.FormulationMillathane 76 100.0Zinc Stearate0.5Poly AC 617A1.0MBTS4.0MBT2.0Thanecure® ZM1.0TP-9510.0Sulfur2.0Hi-Sil 23360All information provided by TSE Industries
Mechanical Properties Metric English Comments
Hardness, Shore A 77
77
Tensile Strength, Yield 13.4 MPa
1950 psi
Elongation at Yield 640 %
640 %
100% Modulus 0.00221 GPa
0.321 ksi
200% Modulus 0.00357 GPa
0.518 ksi
300% Modulus 0.00525 GPa
0.762 ksi
Tear Strength 59.5 kN/m
340 pli
Taber Abrasion, mg/1000 Cycles 23

@Load 1.00 kg
23

@Load 2.20 lb
H-18 wheel
Compression Set 91 %

@Temperature 70.0 °C,
Time 79200 sec
91 %

@Temperature 158 °F,
Time 22.0 hour
Processing Properties Metric English Comments
Cure Time 25.0 min

@Temperature 149 °C
0.417 hour

@Temperature 300 °F