Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

DuPont Teijin Films Melinex® ST339 Polyester Film, 500 Gauge

Category Polymer , Film , Thermoplastic , Polyester, TP , Polyester Film
Manufacturer DuPont Teijin Films (DTF)
Trade Name Melinex®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF DuPont Teijin Films Melinex® ST339 Polyester Film, 500 Gauge.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Melinex® ST339 is a stabilized, opaque white polyester film with good handling and lay flat properties that is pre-treated on both surfaces to promote adhesion to most industrial coatings Typical Applications: Melinex® ST339 is used in applications where the film is exposed to high temperatures and film shrinkage and flatness after the heat exposure is critical.Information provided by DuPont.
Physical Properties Metric English Comments
Density 1.48 g/cc
0.0535 lb/in³
ASTM D1505-85
Mechanical Properties Metric English Comments
Film Tensile Strength at Yield, MD 82.7 MPa
12000 psi
ASTM D882A
Film Tensile Strength at Yield, TD 82.7 MPa
12000 psi
ASTM D882A
Film Elongation at Break, MD 115 %
115 %
ASTM D882A
Film Elongation at Break, TD 90 %
90 %
ASTM D882A
Film Tensile Strength at Break, MD 138 MPa
20000 psi
ASTM D882A
Film Tensile Strength at Break, TD 159 MPa
23000 psi
ASTM D882A
Thermal Properties Metric English Comments
Shrinkage, MD 0.10 %

@Temperature 150 °C,
Time 1800 sec
0.10 %

@Temperature 302 °F,
Time 0.500 hour
Unrestrained
Shrinkage, TD 0.050 %

@Temperature 150 °C,
Time 1800 sec
0.050 %

@Temperature 302 °F,
Time 0.500 hour
Unrestrained
Optical Properties Metric English Comments
Gloss 40 %
40 %
45°; ASTM D1003
45 %
45 %
60°; ASTM D1003
Transmission, Visible 6.0 %
6.0 %
TLT; ASTM D1003
Descriptive Properties Value Comments
Yield (nominal) 4000 in2/lb