Material Notes:
Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).
Physical Properties Metric English Comments
Bulk Density 2.72 g/cc

@Temperature 1000 °C,
Time 10800 sec
0.0983 lb/in³

@Temperature 1830 °F,
Time 3.00 hour
2.74 g/cc

@Temperature 110 °C,
Time 86400 sec
0.0990 lb/in³

@Temperature 230 °F,
Time 24.0 hour
2.78 g/cc

@Temperature 1500 °C,
Time 10800 sec
0.100 lb/in³

@Temperature 2730 °F,
Time 3.00 hour
Porosity 15 %

@Temperature 110 °C,
Time 86400 sec
15 %

@Temperature 230 °F,
Time 24.0 hour
16 %

@Temperature 1500 °C,
Time 10800 sec
16 %

@Temperature 2730 °F,
Time 3.00 hour
19 %

@Temperature 1000 °C,
Time 10800 sec
19 %

@Temperature 1830 °F,
Time 3.00 hour
Mechanical Properties Metric English Comments
Modulus of Rupture 0.0073575 GPa

@Temperature 110 °C,
Time 86400 sec
1.0671 ksi

@Temperature 230 °F,
Time 24.0 hour
0.010791 GPa

@Temperature 1000 °C,
Time 10800 sec
1.5651 ksi

@Temperature 1830 °F,
Time 3.00 hour
0.01913 GPa

@Temperature 1500 °C,
Time 10800 sec
2.775 ksi

@Temperature 2730 °F,
Time 3.00 hour
Thermal Properties Metric English Comments
Shrinkage -0.200 %

@Temperature 1500 °C,
Time 10800 sec
-0.200 %

@Temperature 2730 °F,
Time 3.00 hour
-0.150 %

@Temperature 1000 °C,
Time 10800 sec
-0.150 %

@Temperature 1830 °F,
Time 3.00 hour
-0.0500 %

@Temperature 110 °C,
Time 86400 sec
-0.0500 %

@Temperature 230 °F,
Time 24.0 hour
Component Elements Properties Metric English Comments
Al2O3 79 %
79 %
SiO2 18 %
18 %
Descriptive Properties Value Comments
Main Applications Blast furnace shaft
Material Required for Estimating (kg/?) 2,750