| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.68 g/cc | 0.0607 lb/in³ | ASTM D792 |
| Water Absorption at Saturation | <= 0.10 % | <= 0.10 % | ASTM D570 |
| Linear Mold Shrinkage, Flow | 0.025 cm/cm | 0.025 in/in | |
| Melt Flow | 18 g/10 min <br>@Load 2.16 kg,<br> Temperature 275 °C |
18 g/10 min <br>@Load 4.76 lb,<br> Temperature 527 °F |
ASTM D1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 90 | 90 | ASTM D785 |
| Hardness, Shore D | 75 | 75 | ASTM D2240 |
| Tensile Strength at Break | 47.0 MPa | 6820 psi | 50 mm/min; ASTM D638 |
| Tensile Strength, Yield | 30.0 MPa | 4350 psi | 50 mm/min; ASTM D638 |
| Elongation at Break | 250 % | 250 % | 50 mm/min; ASTM D638 |
| Elongation at Yield | 5.0 % | 5.0 % | 50 mm/min; ASTM D638 |
| Tensile Modulus | 1.66 GPa | 241 ksi | 50 mm/min; ASTM D638 |
| Flexural Strength | 47.0 MPa | 6820 psi | 2.5 mm/min; ASTM D790 |
| Flexural Modulus | 1.69 GPa | 245 ksi | 2.5 mm/min; ASTM D790 |
| Izod Impact, Notched | 2.10 J/cm <br>@Thickness 3.20 mm,<br> Temperature -40.0 °C |
3.93 ft-lb/in <br>@Thickness 0.126 in,<br> Temperature -40.0 °F |
ASTM D256 |
| NB <br>@Thickness 3.20 mm,<br> Temperature 23.0 °C |
NB <br>@Thickness 0.126 in,<br> Temperature 73.4 °F |
ASTM D256 | |
| Coefficient of Friction, Dynamic | 0.20 | 0.20 | vs. Itself; ASTM D1894 |
| Coefficient of Friction, Static | 0.30 | 0.30 | vs. Itself; ASTM D1894 |
| Taber Abrasion, mg/1000 Cycles | 5.0 | 5.0 | CS-17 Wheel, 500 g; ASTM D1044 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 100 µm/m-°C | 55.6 µin/in-°F | |
| Specific Heat Capacity | 0.962 J/g-°C | 0.230 BTU/lb-°F | ASTM C351 |
| Thermal Conductivity | 0.150 W/m-K <br>@Temperature 40.0 °C |
1.04 BTU-in/hr-ft²-°F <br>@Temperature 104 °F |
ASTM C177 |
| Melting Point | 242 °C | 468 °F | DSC |
| Crystallization Temperature | 222 °C | 432 °F | Peak; ASTM D3418 |
| Deflection Temperature at 0.46 MPa (66 psi) | 90.0 °C | 194 °F | Unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 65.0 °C | 149 °F | Unannealed; ASTM D648 |
| Brittleness Temperature | <= -76.0 °C | <= -105 °F | Procedure A; ASTM D746 |
| Glass Transition Temp, Tg | 85.0 °C | 185 °F | ASTM E1356 |
| Flammability, UL94 | V-0 | V-0 | |
| Oxygen Index | 52 % | 52 % | ASTM D2863 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 5.50e+16 ohm-cm | 5.50e+16 ohm-cm | ASTM D257 |
| Dielectric Constant | 2.57 <br>@Frequency 1.00e+6 Hz |
2.57 <br>@Frequency 1.00e+6 Hz |
ASTM D150 |
| Dielectric Strength | 14.0 kV/mm <br>@Thickness 3.18 mm |
356 kV/in <br>@Thickness 0.125 in |
ASTM D149 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Availability | Africa & Middle East | |
| Asia Pacific | ||
| Europe | ||
| Latin America | ||
| North America | ||
| Form | Pellets | |
| Processing Technique | Extrusion; Injection Molding |