| Category | Polymer , Thermoplastic , Polypropylene (PP) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | SABIC PPCOMPOUND |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | SABIC Innovative Plastics SABIC PPCOMPOUND 7450 PP.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 0.970 g/cc | 0.970 g/cc | ASTM D792 |
| Density | 0.970 g/cc | 0.0350 lb/in³ | ISO 1183 |
| Linear Mold Shrinkage, Flow | 0.0069 cm/cm | 0.0069 in/in | 48 hrs @ 23°C, flow; SABIC Method |
| 0.0074 cm/cm | 0.0074 in/in | 1 hr @ 80°C, flow; SABIC Method | |
| Linear Mold Shrinkage, Transverse | 0.010 cm/cm | 0.010 in/in | 48 hrs @ 23°C, xflow; SABIC Method |
| 0.0115 cm/cm | 0.0115 in/in | 1 hr @ 80°C, xflow; SABIC Method | |
| Melt Flow | 21 g/10 min @Load 2.16 kg, Temperature 230 °C |
21 g/10 min @Load 4.76 lb, Temperature 446 °F |
ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 61 | 61 | ISO 868 |
| Tensile Strength at Break | 13.0 MPa | 1890 psi | Type I, 50 mm/min; ASTM D638 |
| 13.0 MPa | 1890 psi | 50 mm/min, 1A; ISO 527 | |
| Tensile Strength, Yield | 15.0 MPa | 2180 psi | Type I, 50 mm/min; ASTM D638 |
| 18.0 MPa | 2610 psi | 50 mm/min; ISO 527 | |
| Elongation at Break | 150 % | 150 % | 50 mm/min; ISO 527 |
| 300 % | 300 % | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Yield | 4.1 % | 4.1 % | 50 mm/min; ISO 527 |
| 9.0 % | 9.0 % | Type I, 50 mm/min; ASTM D638 | |
| Tensile Modulus | 1.12 GPa | 162 ksi | 50 mm/min; ASTM D638 |
| 1.36 GPa | 197 ksi | 1 mm/min; ISO 527 | |
| Flexural Modulus | 1.10 GPa | 160 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
| 1.40 GPa | 203 ksi | 2 mm/min, 64mm span; ISO 178 | |
| Izod Impact, Notched | 4.47 J/cm | 8.37 ft-lb/in | 63.5*12.7*3.2mm, Cut; ASTM D256 |
| Izod Impact, Unnotched | 9.82 J/cm | 18.4 ft-lb/in | 63.5*12.7*3.2mm, Cut; ASTM D4812 |
| Izod Impact, Notched (ISO) | NB | NB | 80*10*4mm, Cut; ISO 180/1A |
| 5.00 kJ/m² @Temperature -30.0 °C |
2.38 ft-lb/in² @Temperature -22.0 °F |
80*10*4mm, Cut; ISO 180/1A | |
| NB @Temperature 0.000 °C |
NB @Temperature 32.0 °F |
80*10*4mm, Cut; ISO 180/1A | |
| Charpy Impact, Notched | NB | NB | 80*10*4mm, Cut; ISO 179/1eA |
| 0.400 J/cm² @Temperature -30.0 °C |
1.90 ft-lb/in² @Temperature -22.0 °F |
80*10*4mm, Cut; ISO 179/1eA | |
| Dart Drop, Total Energy | 14.0 J @Temperature 23.0 °C |
10.3 ft-lb @Temperature 73.4 °F |
Instrumented Impact Energy @ peak, 6.6 m/s; ASTM D3763 |
| 20.0 J @Temperature -30.0 °C |
14.8 ft-lb @Temperature -22.0 °F |
Instrumented Impact Energy @ peak, -30°C @ 2.2 m/s; ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 0.46 MPa (66 psi) | 90.0 °C | 194 °F | 80*10*4mm, Cut; ISO 75-1&2 |
| 79.0 °C @Thickness 3.20 mm |
174 °F @Thickness 0.126 in |
ASTM D648 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 57.0 °C | 135 °F | 80*10*4mm, Cut; ISO 75-1&2 |
| 49.0 °C @Thickness 3.20 mm |
120 °F @Thickness 0.126 in |
ASTM D648 | |
| Vicat Softening Point | 120 °C | 248 °F | 10N, 50°C/hr; ISO 306 |