Material Notes:
PC-siloxane copolymer in special light diffusion colors. Medium flow. Improved toughness compared to medium flow standard PC in same color. Color package may affect performance.
Physical Properties Metric English Comments
Specific Gravity 1.18 g/cc
1.18 g/cc
ASTM D792
Density 1.18 g/cc
0.0426 lb/in³
ISO 1183
Moisture Absorption 0.0900 %
0.0900 %
23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.12 %
0.12 %
ISO 62
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cm
0.0040 - 0.0080 in/in
on Tensile Bar; SABIC Method
0.0040 - 0.0080 cm/cm

@Thickness 3.20 mm
0.0040 - 0.0080 in/in

@Thickness 0.126 in
SABIC Method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0080 cm/cm

@Thickness 3.20 mm
0.0040 - 0.0080 in/in

@Thickness 0.126 in
SABIC Method
Melt Flow 10 g/10 min

@Load 1.20 kg,
Temperature 300 °C
10 g/10 min

@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
Melt Index of Compound 9.0 g/10 min

@Load 1.20 kg,
Temperature 300 °C
9.0 g/10 min

@Load 2.65 lb,
Temperature 572 °F
MVR [cm^3/10 min]; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 51.0 MPa
7400 psi
Type I, 50 mm/min; ASTM D638
54.0 MPa
7830 psi
50 mm/min; ISO 527
Tensile Strength, Yield 57.0 MPa
8270 psi
50 mm/min; ISO 527
59.0 MPa
8560 psi
Type I, 50 mm/min; ASTM D638
Elongation at Break 84 %
84 %
Type I, 50 mm/min; ASTM D638
107 %
107 %
50 mm/min; ISO 527
Elongation at Yield 5.4 %
5.4 %
50 mm/min; ISO 527
5.8 %
5.8 %
Type I, 50 mm/min; ASTM D638
Tensile Modulus 2.24 GPa
325 ksi
50 mm/min; ASTM D638
2.30 GPa
334 ksi
1 mm/min; ISO 527
Flexural Yield Strength 85.0 MPa
12300 psi
1.3 mm/min, 50 mm span; ASTM D790
89.0 MPa
12900 psi
2 mm/min; ISO 178
Flexural Modulus 2.15 GPa
312 ksi
2 mm/min; ISO 178
2.22 GPa
322 ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 8.17 J/cm
15.3 ft-lb/in
ASTM D256
7.21 J/cm

@Temperature -30.0 °C
13.5 ft-lb/in

@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 65.0 kJ/m²
30.9 ft-lb/in²
80*10*3; ISO 180/1A
55.0 kJ/m²

@Temperature -30.0 °C
26.2 ft-lb/in²

@Temperature -22.0 °F
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NB
NB
80*10*3; ISO 180/1U
NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
80*10*3; ISO 180/1U
Charpy Impact Unnotched NB
NB
Edgew 80*10*3 sp=62mm; ISO 179/1eU
NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 7.00 J/cm²
33.3 ft-lb/in²
Edgew 80*10*3 sp=62mm; ISO 179/1eA
6.00 J/cm²

@Temperature -30.0 °C
28.6 ft-lb/in²

@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 76.0 J

@Temperature 23.0 °C
56.1 ft-lb

@Temperature 73.4 °F
ASTM D3763
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 67.0 µm/m-°C

@Temperature -40.0 - 95.0 °C
37.2 µin/in-°F

@Temperature -40.0 - 203 °F
ASTM E 831
67.0 µm/m-°C

@Temperature 23.0 - 80.0 °C
37.2 µin/in-°F

@Temperature 73.4 - 176 °F
ISO 11359-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C

@Temperature -40.0 - 95.0 °C
44.4 µin/in-°F

@Temperature -40.0 - 203 °F
ASTM E 831
80.0 µm/m-°C

@Temperature 23.0 - 80.0 °C
44.4 µin/in-°F

@Temperature 73.4 - 176 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 116 °C
241 °F
Flatw 80*10*4 sp=64mm; ISO 75/Af
122 °C

@Thickness 3.20 mm
252 °F

@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 138 °C
280 °F
Rate B/50; ASTM D1525
138 °C
280 °F
Rate B/50; ISO 306
142 °C
288 °F
Rate B/120; ISO 306
Descriptive Properties Value Comments
Ball Pressure Test, 125°C +/- 2°C pass
IEC 60695-10-2