| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® FXD1414T PC Copolymer (Asia Pacific)
PC-siloxane copolymer in special light diffusion colors. Medium flow. Improved toughness compared to medium flow standard PC in same color. Color package may affect performance.
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1212 PC Copolymer
18 MFR LEXAN High Flow Ductile Copolymer
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1212 PC Copolymer (Europe-Africa-Middle East)
18 MFR LEXAN High Flow Ductile Copolymer
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1232 PC Copolymer
18 MFR LEXAN High Flow Ductile Copolymer UV-stabilized, available in transparent colors only
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1232 PC Copolymer (Asia Pacific)
18 MFR LEXAN High Flow Ductile Copolymer UV-stabilized, available in transparent colors only
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1232 PC Copolymer (Europe-Africa-Middle East)
18 MFR LEXAN High Flow Ductile Copolymer UV-stabilized, available in transparent colors only
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® SLX1432 PC Copolymer
Medium viscosity PC copolymer with enhanced UV stabilization and added release agent. Available in opaque colors. Typical minimum color tolerance limit is DE CMC < 1.0
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® FXD1414T PC Copolymer
PC-siloxane copolymer in special light diffusion colors. Medium flow. Improved toughness compared to medium flow standard PC in same color. Color package may affect performance.
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® HFD1212 PC Copolymer (Asia Pacific)
18 MFR LEXAN High Flow Ductile Copolymer
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® SLX1432 PC Copolymer (Asia Pacific)
Medium viscosity PC copolymer with enhanced UV stabilization and added release agent. Available in opaque colors. Typical minimum color tolerance limit is DE CMC < 1.0
|
|||
| Dart Drop, Total Energy |
76.0
J @Temperature 23.0 °C |
56.1
ft-lb @Temperature 73.4 °F |
ASTM D3763 |
|
SABIC Innovative Plastics Lexan® SLX1432 PC Copolymer (Europe-Africa-Middle East)
Medium viscosity PC copolymer with enhanced UV stabilization and added release agent. Available in opaque colors. Typical minimum color tolerance limit is DE CMC < 1.0
|
|||
| Dart Drop, Total Energy | 76.0 J | 56.1 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRILOY RX05498 PA 66
LNP LUBRILOY* RX05498 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added features of this material include: High Impact, Wear Resistant.
|
|||
| Dart Drop, Total Energy | 76.0 J | 56.1 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRILOY RX05498 PA 66 (Asia Pacific)
LNP LUBRILOY* RX05498 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added features of this material include: High Impact.
|
|||
| Dart Drop, Total Energy | 76.0 J | 56.1 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRILOY RX99650 PA 66
LNP LUBRILOY* RX99650 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added feature of this material is: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 76.0 J | 56.1 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRILOY RX99650 PA 66 (Asia Pacific)
LNP LUBRILOY* RX99650 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added features of this material include: Internally Lubricated.
|
|||
| Dart Drop, Total Energy | 76.0 J | 56.1 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRILOY RX99650 PA 66 (Europe-Africa-Middle East)
LNP LUBRILOY* RX99650 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added features of this material include: Internally Lubricated.
|
|||