Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyester Thermoplastic Elastomer

Category Polymer , Thermoplastic , Elastomer, TPE , Polyester, TP , Polyester Thermoplastic Elastomer
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyester Thermoplastic Elastomer.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyester Thermoplastic Elastomer". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.000657 - 2.10 g/cc
0.0000237 - 0.0759 lb/in³
Average value: 1.16 g/cc Grade Count:154
0.940 - 1.30 g/cc

@Temperature 170 - 240 °C
0.0340 - 0.0470 lb/in³

@Temperature 338 - 464 °F
Average value: 1.04 g/cc Grade Count:27
Water Absorption 0.100 - 12.0 %
0.100 - 12.0 %
Average value: 1.04 % Grade Count:67
Moisture Absorption at Equilibrium 0.0500 - 0.800 %
0.0500 - 0.800 %
Average value: 0.324 % Grade Count:61
Molecular Weight 458 g/mol
458 g/mol
Average value: 458 g/mol Grade Count:21
Maximum Moisture Content 0.0100
0.0100
Average value: 0.0100 Grade Count:28
Linear Mold Shrinkage 0.00200 - 0.0220 cm/cm
0.00200 - 0.0220 in/in
Average value: 0.0118 cm/cm Grade Count:101
Linear Mold Shrinkage, Transverse 0.00400 - 0.0220 cm/cm
0.00400 - 0.0220 in/in
Average value: 0.0130 cm/cm Grade Count:44
Melt Flow 0.400 - 50.0 g/10 min
0.400 - 50.0 g/10 min
Average value: 12.2 g/10 min Grade Count:117
Mechanical Properties Metric English Comments
Hardness, Shore A 65.0 - 99.0
65.0 - 99.0
Average value: 90.7 Grade Count:52
Hardness, Shore D 19.0 - 82.0
19.0 - 82.0
Average value: 49.3 Grade Count:145
Tensile Strength, Ultimate 0.560 - 104 MPa
81.2 - 15100 psi
Average value: 19.1 MPa Grade Count:137
2.53 - 45.81 MPa

@Temperature -40.0 - 160 °C
367 - 6644 psi

@Temperature -40.0 - 320 °F
Average value: 17.3 MPa Grade Count:1
2.53 - 45.81 MPa

@Strain 1.68 - 146 %
367 - 6644 psi

@Strain 1.68 - 146 %
Average value: 17.3 MPa Grade Count:1
Tensile Strength, Yield 2.60 - 72.2 MPa
377 - 10500 psi
Average value: 23.7 MPa Grade Count:77
Elongation at Break 1.90 - 900 %
1.90 - 900 %
Average value: 445 % Grade Count:157
Elongation at Yield 15.0 - 44.0 %
15.0 - 44.0 %
Average value: 30.1 % Grade Count:16
Modulus of Elasticity 0.0130 - 10.5 GPa
1.89 - 1520 ksi
Average value: 0.426 GPa Grade Count:68
0.00163 - 3.14966 GPa

@Temperature -100 - 200 °C
0.236 - 456.827 ksi

@Temperature -148 - 392 °F
Average value: 0.685 GPa Grade Count:20
Flexural Yield Strength 1.00 - 157 MPa
145 - 22800 psi
Average value: 21.3 MPa Grade Count:14
Flexural Modulus 0.0130 - 9.03 GPa
1.89 - 1310 ksi
Average value: 0.356 GPa Grade Count:117
0.00800 - 2.50 GPa

@Temperature -40.0 - 100 °C
1.16 - 363 ksi

@Temperature -40.0 - 212 °F
Average value: 0.758 GPa Grade Count:10
Compressive Modulus 0.00240 - 0.0392 GPa
0.348 - 5.69 ksi
Average value: 0.0153 GPa Grade Count:29
Resilience 40.0 - 81.0
40.0 - 81.0
Average value: 61.3 Grade Count:35
Flex Crack Resistance 1.00e+6
1.00e+6
Average value: 1.00e+6 Grade Count:7
Shear Modulus 0.00640 - 0.307 GPa
0.928 - 44.5 ksi
Average value: 0.0954 GPa Grade Count:12
>= 0.00120 GPa

@Temperature -100 - 200 °C
>= 0.174 ksi

@Temperature -148 - 392 °F
Average value: 0.246 GPa Grade Count:12
Shear Strength 0.0829193 - 0.654548 MPa

@Temperature 230 - 250 °C
12.0264 - 94.9343 psi

@Temperature 446 - 482 °F
Average value: 0.314 MPa Grade Count:1
0.0829193 - 0.654548 MPa

@Shear Rate 50.0 - 5000 1/s
12.0264 - 94.9343 psi

@Shear Rate 50.0 - 5000 1/s
Average value: 0.314 MPa Grade Count:1
Izod Impact, Notched 0.320 J/cm - NB
0.599 ft-lb/in - NB
Average value: 5.39 J/cm Grade Count:70
0.26695 J/cm - NB

@Temperature -40.0 - -40.0 °C
0.50011 ft-lb/in - NB

@Temperature -40.0 - -40.0 °F
Average value: 1.16 J/cm Grade Count:8
0.490332 - 980.567 J/cm

@Temperature -40.0 - -40.0 °C
0.918594 - 1837.00 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 1.16 J/cm Grade Count:27
0.490332 - 980.567 J/cm

@Thickness 6.40 - 6.40 mm
0.918594 - 1837.00 ft-lb/in

@Thickness 0.252 - 0.252 in
Average value: 1.16 J/cm Grade Count:27
Izod Impact, Unnotched 4.80 - 5340 J/cm
8.99 - 10000 ft-lb/in
Average value: 4.80 J/cm Grade Count:3
Izod Impact, Notched (ISO) 3.00 kJ/m² - NB
1.43 ft-lb/in² - NB
Average value: 32.8 kJ/m² Grade Count:28
3.50 kJ/m² - NB

@Temperature -50.0 - -20.0 °C
1.67 ft-lb/in² - NB

@Temperature -58.0 - -4.00 °F
Average value: 10.6 kJ/m² Grade Count:30
Charpy Impact Unnotched 7.10 J/cm² - NB
33.8 ft-lb/in² - NB
Average value: 8.65 J/cm² Grade Count:37
0.450 J/cm² - NB

@Temperature -30.0 - -30.0 °C
2.14 ft-lb/in² - NB

@Temperature -22.0 - -22.0 °F
Average value: 0.450 J/cm² Grade Count:29
Charpy Impact, Notched 0.940 J/cm² - NB
4.47 ft-lb/in² - NB
Average value: 6.67 J/cm² Grade Count:65
0.450 J/cm² - NB

@Temperature -40.0 - -30.0 °C
2.14 ft-lb/in² - NB

@Temperature -40.0 - -22.0 °F
Average value: 5.40 J/cm² Grade Count:46
Tensile Creep Modulus, 1 hour 22.0 - 360 MPa
3190 - 52200 psi
Average value: 132 MPa Grade Count:17
30.7907 - 111.849 MPa

@Temperature 40.0 - 100 °C
4465.82 - 16222.4 psi

@Temperature 104 - 212 °F
Average value: 66.3 MPa Grade Count:1
30.7907 - 111.849 MPa

@Pressure 0.500 - 7.00 MPa
4465.82 - 16222.4 psi

@Pressure 72.5 - 1020 psi
Average value: 66.3 MPa Grade Count:1
Tensile Creep Modulus, 1000 hours 18.0 - 310 MPa
2610 - 45000 psi
Average value: 99.2 MPa Grade Count:17
21.7457 - 83.3376 MPa

@Temperature 40.0 - 100 °C
3153.95 - 12087.1 psi

@Temperature 104 - 212 °F
Average value: 49.2 MPa Grade Count:1
21.7457 - 83.3376 MPa

@Pressure 0.500 - 7.00 MPa
3153.95 - 12087.1 psi

@Pressure 72.5 - 1020 psi
Average value: 49.2 MPa Grade Count:1
Tear Strength 40.0 - 362 kN/m
228 - 2070 pli
Average value: 137 kN/m Grade Count:115
Taber Abrasion, mg/1000 Cycles 5.00 - 90.0
5.00 - 90.0
Average value: 20.7 Grade Count:33
Compression Set 1.00 - 65.0 %
1.00 - 65.0 %
Average value: 41.5 % Grade Count:36
41.0 - 60.0 %

@Temperature 70.0 - 70.0 °C
41.0 - 60.0 %

@Temperature 158 - 158 °F
Average value: 48.8 % Grade Count:11
Torsional Stiffness 20.0 - 500 MPa
2900 - 72500 psi
Average value: 198 MPa Grade Count:11
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+11 - 4.00e+16 ohm-cm
1.00e+11 - 4.00e+16 ohm-cm
Average value: 1.05e+15 ohm-cm Grade Count:72
Surface Resistance 5.00e+12 - 2.00e+17 ohm
5.00e+12 - 2.00e+17 ohm
Average value: 1.55e+16 ohm Grade Count:28
Dielectric Constant 3.30 - 6.80
3.30 - 6.80
Average value: 4.66 Grade Count:29
Dielectric Strength 11.8 - 34.0 kV/mm
300 - 864 kV/in
Average value: 21.6 kV/mm Grade Count:78
Users viewing this material also viewed the following: