Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

LyondellBasell Petrothene® GA808091 Linear Low Density Polyethylene

Category Polymer , Thermoplastic , Polyethylene (PE) , LLDPE
Manufacturer LyondellBasell (former Equistar)
Trade Name Petrothene®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF LyondellBasell Petrothene® GA808091 Linear Low Density Polyethylene.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
ApplicationsPETROTHENE GA 808-091 is a broad molecular weight, linear low density polyethylene resin designed for use as a base resin in wire and cable jacketing. An antioxidant package is added to ensure thermal stability during processing.Processing TechniquesGA 808-091, like other thermoplastic polyolefin resins, can be extruded as wire and cable insulation using a conventional extruder. Below are suggested extrusion conditions for GA 808-091. These conditions are intended as general guidelines only and are not optimum values, since manufacturing conditions, such as extruder type and size have an effect on the processing of thermoplastic resins.Industry SpecificationsGA 808-091 meets the requirements of the following: ASTM D1248, Type 1, Category 4, Class A, Grade E5. Federal LP390C, Type II, Class L, Category 4, Grade 4.This product is from the former Equistar product line.
Physical Properties Metric English Comments
Density 0.920 g/cc
0.0332 lb/in³
ASTM D1505
Environmental Stress Crack Resistance >= 1000 hour
>= 1000 hour
10% Igepal®, F<sub>50</sub>; ASTM D1693
Melt Flow 0.75 g/10 min
0.75 g/10 min
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Shore D 57
57
ASTM D2240
Tensile Strength at Break 15.2 MPa
2200 psi
ASTM D638
Tensile Strength, Yield 11.7 MPa
1700 psi
ASTM D638
Elongation at Break 650 %
650 %
ASTM D638
1% Secant Modulus 345 MPa
50000 psi
ASTM D790
Thermal Properties Metric English Comments
Brittleness Temperature <= -76.0 °C
<= -105 °F
F<sub>50</sub>; ASTM D746
Electrical Properties Metric English Comments
Dielectric Constant 2.29
2.29
ASTM D1531
Dissipation Factor 0.000060
0.000060
ASTM D1531
Processing Properties Metric English Comments
Feed Temperature 154 - 163 °C
310 - 325 °F
Zone 2 177 - 193 °C
350 - 380 °F
Zone 3 193 - 210 °C
380 - 410 °F
Zone 4-x 204 - 218 °C
400 - 425 °F
Adapter Temperature 204 - 218 °C
400 - 425 °F
Die Temperature 204 - 218 °C
400 - 425 °F
Copyright © lookpolymers.com All Rights Reserved