Ensinger Delrin® 150 Homopolymer Acetal (POM)

Category Polymer , Thermoplastic , Acetal (POM) , Acetal Homopolymer, Unreinforced
Manufacturer Ensinger
Trade Name Delrin®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Ensinger Delrin® 150 Homopolymer Acetal (POM).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Ensinger's Delrin® 150 stock shapes are a homopolymer acetal manufactured using DuPont Delrin 150 Resin. It is a crystalline plastic which offers an excellent balance of properties to bridge the gap between metals and plastics. It possesses high tensile and flexural properties, along with creep resistance and toughness, while exhibiting low moisture absorption, and fatigue endurance.
Physical Properties Metric English Comments
Specific Gravity 1.42 g/cc
1.42 g/cc
ASTM D792
Water Absorption 0.25 %

@Time 86400 sec
0.25 %

@Time 24.0 hour
ASTM D570
Water Absorption at Saturation 0.90 %
0.90 %
ASTM D570
Mechanical Properties Metric English Comments
Hardness, Rockwell M 94
94
ASTM D785
Hardness, Rockwell R 120
120
ASTM D785
Tensile Strength, Yield 75.8 MPa
11000 psi
ASTM D638
Elongation at Break 25 %
25 %
ASTM D638
Tensile Modulus 3.10 GPa
450 ksi
ASTM D638
Flexural Strength 110 MPa
16000 psi
ASTM D790
Flexural Modulus 2.90 GPa
420 ksi
ASTM D790
Compressive Strength 35.9 MPa
5200 psi
ASTM D695
Izod Impact, Unnotched 0.80 J/cm
1.5 ft-lb/in
ASTM D256
Coefficient of Friction, Dynamic 0.20
0.20
40 psi, 50 fpm; ASTM D3702
K (wear) Factor 111 x 10-8 mm³/N-M
55.0 x 10-10 in³-min/ft-lb-hr
ASTM D3702
Limiting Pressure Velocity 0.0513 MPa-m/sec
1460 psi-ft/min
ASTM D792
Thermal Properties Metric English Comments
CTE, linear 122 µm/m-°C
68.0 µin/in-°F
ASTM D696
Melting Point 175 °C
347 °F
ASTM D2133
Maximum Service Temperature, Air 85.0 °C
185 °F
Continuous; UL746B
149 °C
300 °F
Intermittent
Deflection Temperature at 0.46 MPa (66 psi) 169 °C
336 °F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 125 °C
257 °F
ASTM D648
Flammability, UL94 HB
HB
UL 94
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+15 ohm-cm
1.00e+15 ohm-cm
ASTM D257
Dielectric Constant 3.7

@Frequency 60.0 Hz
3.7

@Frequency 60.0 Hz
50% RH; ASTM D150
Dielectric Strength 19.7 kV/mm
500 kV/in
ASTM D149
Dissipation Factor 0.0050

@Frequency 60.0 Hz
0.0050

@Frequency 60.0 Hz
ASTM D150