Eastman DuraStar DS1900HF Polymer, Natural

Category Polymer , Thermoplastic , Polyester, TP , Polycyclohexylenedimethylene Terephthalate (PCT) , Glycol-Modified PCT (PCTG) Copolyester
Manufacturer Eastman Chemical
Trade Name DuraStar
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Eastman DuraStar DS1900HF Polymer, Natural.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Durastar DS1900HF polymer is a high flow grade of Durastar . Durastar DS1900HF flow lengths are increased 20-40% relative to Durastar DS1000 as shown by spiral flow testing. Other outstanding features of Durastar are easily maintained such as excellent appearance and clarity, good physical properties, chemical resistance, and easy processing. This high flow product is especially suited for those applications utilizing thin-walled intricate tools. Under existing United States Food and Drug Administration (FDA) regulations, Durastar DS1900HF may be used in food contact articles which comply with the specifications and conditions of use in 21 CFR 177.1240.Applications/UsesAppliancesFurniture/Furniture trimToys/Sporting goodsFloor careHousewaresWriting instrumentsKey AttributesGood chemical resistanceExcellent flowOutstanding impact resistanceExcellent clarityFast drying timesQuick cycle times
Physical Properties Metric English Comments
Specific Gravity 1.19 g/cc
1.19 g/cc
ASTM D792
Water Absorption 0.15 %
0.15 %
24h Immersion; ASTM D570
Linear Mold Shrinkage 0.0030 cm/cm
0.0030 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 107
107
ASTM D785
Tensile Strength at Break 43.0 MPa
6240 psi
ASTM D638
Tensile Strength, Yield 50.0 MPa
7250 psi
ASTM D638
Elongation at Break 270 %
270 %
ASTM D638
Elongation at Yield 5.0 %
5.0 %
ASTM D638
Flexural Yield Strength 68.0 MPa
9860 psi
ASTM D790
Flexural Modulus 1.90 GPa
276 ksi
ASTM D790
Izod Impact, Notched 0.440 J/cm

@Temperature -40.0 °C
0.824 ft-lb/in

@Temperature -40.0 °F
ASTM D256
0.800 J/cm

@Temperature 23.0 °C
1.50 ft-lb/in

@Temperature 73.4 °F
ASTM D256
Izod Impact, Unnotched NB
NB
ASTM D4812
NB

@Temperature -40.0 °C
NB

@Temperature -40.0 °F
ASTM D4812
Puncture Energy 40.0 J
29.5 ft-lb
Puncture Resistance @Max Load, 23°C; ASTM D3763
38.0 J

@Temperature -40.0 °C
28.0 ft-lb

@Temperature -40.0 °F
Puncture Resistance at Max Load; ASTM D3763
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 73.0 °C
163 °F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 66.0 °C
151 °F
ASTM D648
Vicat Softening Point 86.0 °C
187 °F
1kg load; ASTM D1525
Optical Properties Metric English Comments
Haze <= 1.0 %
<= 1.0 %
ASTM D1003
Transmission, Visible 92 %
92 %
Total Transmittance; ASTM D1003
Processing Properties Metric English Comments
Melt Temperature 230 - 280 °C
446 - 536 °F
Mold Temperature 15.0 - 30.0 °C
59.0 - 86.0 °F
Drying Temperature 70.0 °C
158 °F
Dry Time 4 hour
4 hour