Material Notes:
Product description: Grilon TSZ 3 is a heat stabilized, normal viscosity, high impact modified PA66 + PA6 injection molding grade. Grilon TSZ 3 has the following important properties: Excellent toughnessGood flow behaviorEasy processing Grilon TSZ 3 is used typically for automotive and electro applications such as clips, fixing parts, and cable binders.Information provided by EMS Grivory
Physical Properties Metric English Comments
Density 1.07 g/cc
0.0387 lb/in³
ISO 1183
Water Absorption 7.0 %
7.0 %
ISO 62
Moisture Absorption 2.30 %
2.30 %
ISO 62
Linear Mold Shrinkage, Flow 0.016 cm/cm
0.016 in/in
ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.018 cm/cm
0.018 in/in
ISO 294-4, 2577
Mechanical Properties Metric English Comments
Ball Indentation Hardness 45.0 MPa
6530 psi
conditioned; ISO 2039-1
90.0 MPa
13100 psi
dry; ISO 2039-1
Tensile Stress 30.0 MPa

@Strain 50.0 %
4350 psi

@Strain 50.0 %
conditioned; ISO 527-1/-2
Tensile Strength, Yield 40.0 MPa
5800 psi
dry; ISO 527-1/-2
40.0 MPa
5800 psi
dry; ISO 527-1/-2
Elongation at Break >= 50 %
>= 50 %
dry; ISO 527-1/-2
>= 50 %
>= 50 %
conditioned; ISO 527-1/-2
<= 50 %
<= 50 %
dry; ISO 527-1/-2
Elongation at Yield 5.0 %
5.0 %
dry; ISO 527-1/-2
5.0 %
5.0 %
dry; ISO 527-1/-2
Tensile Modulus 0.550 GPa
79.8 ksi
conditioned; ISO 527-1/-2
1.60 GPa
232 ksi
dry; ISO 527-1/-2
Charpy Impact Unnotched NB
NB
dry; ISO 179/1eU
NB
NB
conditioned; ISO 179/1eU
NB

@Temperature 30.0 °C
NB

@Temperature 86.0 °F
dry; ISO 179/1eU
NB

@Temperature 30.0 °C
NB

@Temperature 86.0 °F
conditioned; ISO 179/1eU
Charpy Impact, Notched 7.00 J/cm²
33.3 ft-lb/in²
dry; ISO 179/1eA
NB
NB
conditioned; ISO 179/1eA
1.50 J/cm²

@Temperature 30.0 °C
7.14 ft-lb/in²

@Temperature 86.0 °F
dry; ISO 179/1eU
1.50 J/cm²

@Temperature 30.0 °C
7.14 ft-lb/in²

@Temperature 86.0 °F
conditioned; ISO 179/1eU
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 120 µm/m-°C
66.7 µin/in-°F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 150 µm/m-°C
83.3 µin/in-°F
ISO 11359-1/-2
Melting Point 260 °C
500 °F
10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 80.0 - 100 °C
176 - 212 °F
long term; EMS
180 °C
356 °F
short term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 140 °C
284 °F
ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C
131 °F
ISO 75-1/-2
Flammability, UL94 HB
HB
IEC 60695-11-10
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+12 ohm-cm
1.00e+12 ohm-cm
conditioned; IEC 60093
1.00e+14 ohm-cm
1.00e+14 ohm-cm
dry; IEC 60093
Surface Resistance 1.00e+11 ohm
1.00e+11 ohm
IEC 60093
Dielectric Strength 30.0 kV/mm
762 kV/in
conditioned; IEC 60243-1
34.0 kV/mm
864 kV/in
dry; IEC 60243-1
Comparative Tracking Index 600 V
600 V
conditioned; IEC 60112
Descriptive Properties Value Comments
Automotive Automotive electr. and electronics, lighting
Electricals & Electronics Connectors
Form Granules
Industry & Consumer goods Mechanical Engineering