Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
PolyOne Geon™ 81530 Polyvinyl Chloride, Rigid (PVC, Rigid) Information provided by PolyOne |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | Below Tg, Result based on 450GL30; ISO 11359 |
Victrex® PEEK 450GL30 Polyetheretherketone, 30% Glass Fiber, Black Product Description: High performance thermoplastic material, 30% glass fiber reinforced PolyEtherEtherKetone (PEEK), semi crystalline, granules for injection moulding and extrusion, Standard viscos.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
10.0 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 |
SABIC Innovative Plastics LNP LUBRICOMP JFL36 PES (Europe-Africa-Middle East) LNP* Lubricomp* JFL36 is a compound based on Polyethersulfone resin containing Glass Fiber, PTFE. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature -30.0 - 30.0 °C |
10.0 µin/in-°F @Temperature -22.0 - 86.0 °F |
ASTM D696 |
SABIC Innovative Plastics LNP LUBRICOMP LX91475 PEEK LNP* LUBRICOMP* LX91475 is a compound based on Polyetheretherketone resin containing proprietary fillers. Added features of this material include: Easy Molding, High Temperature Bearing Grade, Wear.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Elastoblend® PA6 GF18 IM 511 18% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 18% Filler by WeightAdditive: Heat Stabilizer, Impact Modifier and LubricantFeatures: Heat Stabilized, Impac.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Elastoblend® PA6 GF20 IM2 BK 20% Glass Filled (Dry) Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 20% Filler by WeightAdditive: Heat Stabilizer, Impact Modifier and LubricantFeatures: Heat Stabilized, Impac.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ISO 11359-2 |
Solvay Specialty Polymers Ixef® 2030 Polyarylamide (PARA), 55% GlassMineral Ixef® 2030 is a 55% glass-fiber/mineral reinforced polyarylamide compound which exhibits high strength, very high stiffness, low warpage, excellent creep resistance and outstanding surface gloss... |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
10.0 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 |
SABIC Innovative Plastics LNP STAT-KON DEL329EP PC (Europe-Africa-Middle East) LNP* STATKON* DEL329EP is a compound based on Polycarbonate resin containing Carbon Fiber, PTFE, Flame Retardant. Added features include: Electrically Conductive, Internally Lubricated, Flame retard.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill FR® TPX-PBT-00014 40% Glass/Mineral Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass/Mineral, 40% Filler by WeightFeatures: Flame RetardantUL File Number: E157318Information provided by TP Composites, Inc. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill FR® TPX-PBT-01006 40% Glass/Ceramic Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass/Ceramic, 40% Filler by WeightFeatures: Flame RetardantUL File Number: E157318Information provided by TP Composites, Inc. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill® PA6/6 GF/M35 HS BK 35% Glass/Mineral Fiber Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 35% Filler by Weight and Mineral Filler, 35% Filler by WeightAdditive: Lubricant and Heat StabilizerFeatures.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill® PA6/6 GF40 HS L 40% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 40% Filler by WeightAdditive: Lubricant and Heat StabilizerFeatures: Lubricated and Heat StabilizedInformati.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill® PA6/6 GF40 HS L BK 40% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 40% Filler by WeightAdditive: Lubricant and Heat StabilizerFeatures: Lubricated and Heat StabilizedUL File N.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Luriblend® PA6/6 GF33 TL10 HS 33% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 33% Filler by WeightAdditive: Heat Stabilizer and PTFE Lubricant(10%)Features: Lubricated, Good Wear Resistance, Heat Stab.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Luriblend® PA6/6 GF33 TL10 HS BK 33% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 33% Filler by WeightAdditive: Heat Stabilizer and PTFE Lubricant(10%)Features: Lubricated, Good Wear Resistance, Heat Stab.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Luriblend® PA6/6 GF33 TL15 BK 33% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 33% Filler by WeightAdditive: Heat Stabilizer and PTFE Lubricant(15%)Features: Lubricated, Good Wear Resistance, Heat Stab.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Luriblend® PA6/6 GF33 TS15 BK 33% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 33% Filler by WeightAdditive: Heat Stabilizer, Silicone Lubricant and PTFE Lubricant(15%)Features: Lubricated, Good Wear R.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Statiblend® PA6 GF20 AS BK 20% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 20% Filler by WeightAdditive: Antistatic, Heat Stabilizer and LubricantFeatures: Antistatic, Heat Stabilizer and Lubricate.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Statiblend® PA6/6 GF20 AS BK 20% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber, 20% Filler by WeightAdditive: Lubricant, Antistatic and Heat StabilizerFeatures: Antistatic, Heat Stabilized and Lubricate.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
10.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
SABIC Innovative Plastics LNP VERTON MV006S PP (Asia Pacific) LNP VERTON* MV006S is a compound based on Polypropylene resin containing Long Glass. Added features of this material include: Chemically Coupled. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
10.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
SABIC Innovative Plastics LNP VERTON MV006S PP (Europe-Africa-Middle East) LNP VERTON* MV006S is a compound based on Polypropylene resin containing Long Glass. Added features of this material include: Chemically Coupled. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES Elastoblend® PA6 GF20 IM2 L 20% Glass Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 20% Filler by WeightAdditive: Impact Modifier and LubricantFeatures: Impact Modified and LubricatedTPCI# 633.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill® PA4/6 GF25 HS NAT 25% Glass Filled (Dry) Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 25% Filler by WeightAdditive: Heat StabilizerFeatures: Heat StabilizedAppearance: Natural ColorInformation p.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | ASTM D696 |
Techmer ES HiFill® PPS F GF/M55 BK 55% Glass/Mineral Filled Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass/Mineral, 55% Filler by WeightAppearance: BlackInformation provided by TP Composites, Inc. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature 20.0 °C |
10.0 µin/in-°F @Temperature 68.0 °F |
ISO 11359-1/-2 |
DSM Akulon® K224-LGM35 (Dry) 15% Glass Reinforced, 25% Mineral Reinforced Nylon 6 (North America) Description: The Akulon portfolio is engineered for optimum performance to suit different processing techniques and end use markets.Unfilled Extrusion ResinsAkulon resins are available with melt vis.. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | DAM; ISO 11359-1/-2 |
DuPont Performance Polymers Zytel® 70G33HS1L BK031 Nylon 66
(Unverified Data**) 33% Glass Reinforced Heat Stabilized Polyamide 66 Zytel 70G33HS1L BK031 is a 33% glass fiber reinforced heat stabilized black polyamide 66 resin for injection molding.Information provided by DuPont .. |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C | 10.0 µin/in-°F | DAM; ISO 11359-1/-2 |
DuPont Performance Polymers Zytel® 70G33L BK031 Nylon 66
(Unverified Data**) 33% Glass Reinforced Polyamide 66Zytel 70G33L BK031 is a 33% glass fiber reinforced black polyamide 66 resin for injection molding.Information provided by DuPont Performance Polymers |
|||
CTE, linear, Parallel to Flow | 18.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
10.0 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 |
Eurostar Starflam BFR460B PA6, Glass Fiber Filled, Flame Retardant, Injection Molded Starflam BFR460B is a Flame Retardant, Glass Fiber Reinforced Polyamide 6, Injection Molding ResinInformation provided by Eurostar. |