Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 6, 50% Glass Fiber Filled

Category Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 50% Glass Fiber Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 6, 50% Glass Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, 50% Glass Fiber Filled". Specific grades with glass content between 45% and 54% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.30 - 1.80 g/cc
0.0470 - 0.0650 lb/in³
Average value: 1.56 g/cc Grade Count:202
1.24 - 1.33 g/cc

@Temperature 270 - 290 °C
0.0448 - 0.0480 lb/in³

@Temperature 518 - 554 °F
Average value: 1.29 g/cc Grade Count:2
Filler Content 45.0 - 60.0 %
45.0 - 60.0 %
Average value: 49.9 % Grade Count:54
Water Absorption 0.200 - 5.10 %
0.200 - 5.10 %
Average value: 2.24 % Grade Count:85
1.20 - 1.60 %

@Temperature 70.0 - 70.0 °C
1.20 - 1.60 %

@Temperature 158 - 158 °F
Average value: 1.28 % Grade Count:6
Moisture Absorption at Equilibrium 0.250 - 4.80 %
0.250 - 4.80 %
Average value: 1.35 % Grade Count:67
0.450 - 1.00 %

@Temperature 70.0 - 70.0 °C
0.450 - 1.00 %

@Temperature 158 - 158 °F
Average value: 0.717 % Grade Count:1
0.450 - 1.00 %

@Time 180000 - 1.44e+6 sec
0.450 - 1.00 %

@Time 50.0 - 400 hour
Average value: 0.717 % Grade Count:1
Water Absorption at Saturation 3.90 - 8.00 %
3.90 - 8.00 %
Average value: 4.72 % Grade Count:28
Viscosity 100 - 400 cP

@Temperature 230 - 270 °C
100 - 400 cP

@Temperature 446 - 518 °F
Average value: 212 cP Grade Count:1
100 - 400 cP

@Shear Rate 100 - 1000 1/s
100 - 400 cP

@Shear Rate 100 - 1000 1/s
Average value: 212 cP Grade Count:1
Viscosity Test 140 - 150 cm³/g
140 - 150 cm³/g
Average value: 143 cm³/g Grade Count:3
Maximum Moisture Content 0.100
0.100
Average value: 0.100 Grade Count:14
Linear Mold Shrinkage 0.000200 - 0.0350 cm/cm
0.000200 - 0.0350 in/in
Average value: 0.00317 cm/cm Grade Count:150
0.00200 - 0.00200 cm/cm

@Temperature 80.0 - 80.0 °C
0.00200 - 0.00200 in/in

@Temperature 176 - 176 °F
Average value: 0.00200 cm/cm Grade Count:6
Linear Mold Shrinkage, Transverse 0.000500 - 0.0141 cm/cm
0.000500 - 0.0141 in/in
Average value: 0.00707 cm/cm Grade Count:76
0.00600 - 0.00600 cm/cm

@Temperature 80.0 - 80.0 °C
0.00600 - 0.00600 in/in

@Temperature 176 - 176 °F
Average value: 0.00600 cm/cm Grade Count:6
Melt Flow 1.00 - 38.8 g/10 min
1.00 - 38.8 g/10 min
Average value: 16.8 g/10 min Grade Count:14
Spiral Flow 34.0 - 50.0 cm
13.4 - 19.7 in
Average value: 43.8 cm Grade Count:12
Mechanical Properties Metric English Comments
Hardness, Rockwell R 65.0 - 124
65.0 - 124
Average value: 119 Grade Count:34
Hardness, Shore D 78.0 - 98.0
78.0 - 98.0
Average value: 87.5 Grade Count:10
Ball Indentation Hardness 140 - 290 MPa
20300 - 42100 psi
Average value: 237 MPa Grade Count:20
Tensile Strength, Ultimate 25.0 - 605 MPa
3630 - 87700 psi
Average value: 196 MPa Grade Count:148
55.0 - 321.64 MPa

@Temperature -40.0 - 150 °C
7980 - 46650 psi

@Temperature -40.0 - 302 °F
Average value: 139 MPa Grade Count:4
115 - 180 MPa

@Temperature 70.0 - 175 °C
16700 - 26100 psi

@Temperature 158 - 347 °F
Average value: 139 MPa Grade Count:4
115 - 180 MPa

@Time 180000 - 7.20e+7 sec
16700 - 26100 psi

@Time 50.0 - 20000 hour
Average value: 139 MPa Grade Count:4
Tensile Strength, Yield 150 - 240 MPa
21800 - 34800 psi
Average value: 202 MPa Grade Count:48
Elongation at Break 1.00 - 8.00 %
1.00 - 8.00 %
Average value: 3.10 % Grade Count:178
2.30 - 9.00 %

@Temperature 4.44 - 150 °C
2.30 - 9.00 %

@Temperature 40.0 - 302 °F
Average value: 4.76 % Grade Count:3
Elongation at Yield 1.00 - 4.50 %
1.00 - 4.50 %
Average value: 2.65 % Grade Count:10
Modulus of Elasticity 0.0130 - 30.1 GPa
1.89 - 4370 ksi
Average value: 13.7 GPa Grade Count:136
3.80 - 18.25 GPa

@Temperature -40.0 - 150 °C
551 - 2647 ksi

@Temperature -40.0 - 302 °F
Average value: 10.1 GPa Grade Count:5
13.5 - 15.0 GPa

@Temperature 70.0 - 70.0 °C
1960 - 2180 ksi

@Temperature 158 - 158 °F
Average value: 10.1 GPa Grade Count:1
13.5 - 15.0 GPa

@Time 180000 - 1.44e+6 sec
1960 - 2180 ksi

@Time 50.0 - 400 hour
Average value: 10.1 GPa Grade Count:1
Flexural Yield Strength 175 - 840 MPa
25400 - 122000 psi
Average value: 310 MPa Grade Count:127
100 - 433.06 MPa

@Temperature -40.0 - 121 °C
14500 - 62810 psi

@Temperature -40.0 - 250 °F
Average value: 243 MPa Grade Count:3
Flexural Modulus 0.910 - 147 GPa
132 - 21300 ksi
Average value: 13.8 GPa Grade Count:136
4.50 - 15.4443 GPa

@Temperature -40.0 - 121 °C
653 - 2240.03 ksi

@Temperature -40.0 - 250 °F
Average value: 9.91 GPa Grade Count:3
Compressive Yield Strength 160 - 274 MPa
23200 - 39700 psi
Average value: 208 MPa Grade Count:5
Shear Modulus >= 0.528 GPa

@Temperature -50.0 - 200 °C
>= 76.6 ksi

@Temperature -58.0 - 392 °F
Average value: 1.35 GPa Grade Count:1
Izod Impact, Notched 0.908 - 4.97 J/cm
1.70 - 9.30 ft-lb/in
Average value: 2.10 J/cm Grade Count:60
1.15 - 5.97968 J/cm

@Temperature -40.0 - 121 °C
2.15 - 11.2024 ft-lb/in

@Temperature -40.0 - 250 °F
Average value: 2.55 J/cm Grade Count:2
1.01441 - 1.01441 J/cm

@Temperature -40.0 - -40.0 °C
1.90041 - 1.90041 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 2.55 J/cm Grade Count:1
1.01441 - 1.01441 J/cm

@Thickness 3.17 - 3.17 mm
1.90041 - 1.90041 ft-lb/in

@Thickness 0.125 - 0.125 in
Average value: 2.55 J/cm Grade Count:1
Izod Impact, Unnotched 1.39 - 5340 J/cm
2.60 - 10000 ft-lb/in
Average value: 11.7 J/cm Grade Count:35
Izod Impact, Notched (ISO) 12.0 - 147 kJ/m²
5.71 - 69.8 ft-lb/in²
Average value: 20.8 kJ/m² Grade Count:50
11.0 - 20.0 kJ/m²

@Temperature -40.0 - -20.0 °C
5.23 - 9.52 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 14.6 kJ/m² Grade Count:17
Izod Impact, Unnotched (ISO) 70.0 kJ/m² - NB
33.3 ft-lb/in² - NB
Average value: 89.9 kJ/m² Grade Count:19
75.0 kJ/m² - NB

@Temperature -30.0 - -30.0 °C
35.7 ft-lb/in² - NB

@Temperature -22.0 - -22.0 °F
Average value: 88.7 kJ/m² Grade Count:10
Charpy Impact Unnotched 1.50 J/cm² - NB
7.14 ft-lb/in² - NB
Average value: 9.27 J/cm² Grade Count:116
1.40 - 999.9 J/cm²

@Temperature -40.0 - 30.0 °C
6.66 - 4759 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 8.05 J/cm² Grade Count:68
Charpy Impact, Notched 0.600 - 4.00 J/cm²
2.86 - 19.0 ft-lb/in²
Average value: 2.02 J/cm² Grade Count:113
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved