Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Techmer ES HiFill® PA4/6 GF50 HS BK 50% Glass Filled

Category Polymer , Thermoplastic , Nylon , Nylon 46 , Nylon 46, Glass Fiber Reinforced
Manufacturer Techmer ES
Trade Name HiFill®
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Techmer ES HiFill® PA4/6 GF50 HS BK 50% Glass Filled.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 50% Filler by WeightAdditive: Heat StabilizerFeatures: Heat StabilizedAppearance: BlackUL File Number: E157318Information provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.62 g/cc
0.0585 lb/in³
ASTM D792
Water Absorption 1.2 %

@Time 86400 sec
1.2 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0040 cm/cm

@Thickness 3.17 mm
0.0040 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength, Yield 165 MPa
24000 psi
ASTM D638
Elongation at Break 5.0 %
5.0 %
ASTM D638
Flexural Strength 214 MPa
31000 psi
ASTM D790
Flexural Modulus 9.65 GPa
1400 ksi
ASTM D790
Izod Impact, Notched 1.92 J/cm

@Thickness 3.17 mm
3.60 ft-lb/in

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 59.4 µm/m-°C
33.0 µin/in-°F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 285 °C
545 °F
Unannealed; ASTM D648
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+12 ohm-cm
1.00e+12 ohm-cm
ASTM D257
Dielectric Strength 27.6 kV/mm
700 kV/in
Method A (Short-Time); ASTM D149