Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Techmer ES HiFill FR® PA6 FR NAT

Category Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, Unreinforced
Manufacturer Techmer ES
Trade Name HiFill FR®
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Techmer ES HiFill FR® PA6 FR NAT.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Availability: North AmericaForms: PelletsFeatures: Flame Retardant UL File Number: E157318Appearance: Natural ColorProcessing Method: Injection MoldingInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.19 g/cc
0.0430 lb/in³
ASTM D792
Water Absorption 0.70 %

@Time 86400 sec
0.70 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.010 cm/cm

@Thickness 3.17 mm
0.010 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 112
112
ASTM D785
Tensile Strength, Yield 51.7 MPa
7500 psi
ASTM D638
Elongation at Break 60 %
60 %
ASTM D638
Flexural Modulus 1.31 GPa
190 ksi
ASTM D790
Izod Impact, Notched 1.33 J/cm

@Thickness 3.17 mm
2.50 ft-lb/in

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 59.4 µm/m-°C
33.0 µin/in-°F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C
140 °F
Unannealed; ASTM D648
Flammability, UL94 V-0
V-0
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+14 ohm-cm
1.00e+14 ohm-cm
ASTM D257
Surface Resistance 1.00e+12 ohm
1.00e+12 ohm
ASTM D257
Dielectric Strength 20.9 kV/mm
530 kV/in
Method A (Short-Time); ASTM D149
Users viewing this material also viewed the following: