| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.03 g/cc | 0.290 lb/in³ |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell B | 86 | 86 | |
| Tensile Strength, Ultimate | 689 MPa | 100000 psi | |
| Tensile Strength, Yield | 331 MPa <br>@Strain 0.200 % |
48000 psi <br>@Strain 0.200 % |
|
| Elongation at Break | >= 42 % | >= 42 % | in 2 in (50 mm) or 4D |
| Modulus of Elasticity | 188 GPa | 27300 ksi | for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ] |
| Poissons Ratio | 0.33 | 0.33 | |
| Shear Modulus | 77.0 GPa | 11200 ksi |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 15.18 µm/m-°C <br>@Temperature 25.0 - 100 °C |
8.433 µin/in-°F <br>@Temperature 77.0 - 212 °F |
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ] |
| 16.03 µm/m-°C <br>@Temperature 25.0 - 300 °C |
8.906 µin/in-°F <br>@Temperature 77.0 - 572 °F |
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ] | |
| 16.56 µm/m-°C <br>@Temperature 25.0 - 500 °C |
9.200 µin/in-°F <br>@Temperature 77.0 - 932 °F |
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ] | |
| 17.18 µm/m-°C <br>@Temperature 25.0 - 700 °C |
9.544 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ] | |
| Specific Heat Capacity | 0.500 J/g-°C | 0.120 BTU/lb-°F | |
| Thermal Conductivity | 11.5 W/m-K | 79.8 BTU-in/hr-ft²-°F | |
| Melting Point | 1320 - 1400 °C | 2410 - 2550 °F | |
| Solidus | 1320 °C | 2410 °F | |
| Liquidus | 1400 °C | 2550 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Carbon, C | <= 0.20 % | <= 0.20 % | |
| Chromium, Cr | 19 - 21 % | 19 - 21 % | |
| Copper, Cu | 0.50 - 1.5 % | 0.50 - 1.5 % | |
| Iron, Fe | 47.3 % | 47.3 % | As remainder |
| Manganese, Mn | <= 2.0 % | <= 2.0 % | |
| Molybdenum, Mo | 6.0 - 7.0 % | 6.0 - 7.0 % | |
| Nickel, Ni | 24 - 26 % | 24 - 26 % | |
| Nitrogen, N | 0.15 - 0.25 % | 0.15 - 0.25 % | |
| Phosphorous, P | <= 0.030 % | <= 0.030 % | |
| Silicon, Si | <= 0.50 % | <= 0.50 % | |
| Sulfur, S | <= 0.010 % | <= 0.010 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.0000800 ohm-cm | 0.0000800 ohm-cm | |
| Magnetic Permeability | 1.005 | 1.005 | at 200 Oersted (15.9 kA/m) |