Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers Amodel® AFA-6133 V0 Z Polyphthalamide (PPA), 33% Glass Fiber (Conditioned)

Category Polymer , Thermoplastic , Polyphthalamide (PPA) , Polyphthalamide (PPA), 30% Glass Fiber Reinforced
Manufacturer Solvay Specialty Polymers
Trade Name Amodel®
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Solvay Specialty Polymers Amodel® AFA-6133 V0 Z Polyphthalamide (PPA), 33% Glass Fiber (Conditioned).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Amodel® AFA-6133 V0 Z is a 33% glass-fiber reinforced, flame retardant grade of polyphthalamide (PPA) resin specifically formulated for connector applications requiring compatibility with both infrared and vapor phase soldering operations typically used by the electronics industry.Features: Flame Retardant; Good Chemical Resistance; Good Dimensional Stability; Good Electrical Properties; Good Stiffness; High Flow; High Strength; Hot Water MoldabilityUses: Automotive Applications; Automotive Electronics; Bobbins; Connectors; Electrical/Electronic ApplicationsInjection Molding Notes: Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding.Automotive Specifications ASTM D6779 PA104G35; GM GMW15702 Color: BK BlackInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Density 1.68 g/cc
0.0607 lb/in³
Dry; ISO 1183
Filler Content 33 %
33 %
Glass Fiber
Linear Mold Shrinkage, Flow 0.0030 cm/cm
0.0030 in/in
Dry
Linear Mold Shrinkage, Transverse 0.0060 cm/cm
0.0060 in/in
Dry; ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength 166 MPa
24100 psi
ASTM D638
Tensile Strength, Yield 63.4 MPa
<br>@Temperature 175 °C
9200 psi
<br>@Temperature 347 °F
4; ISO 527-2
75.2 MPa
<br>@Temperature 150 °C
10900 psi
<br>@Temperature 302 °F
4; ISO 527-2
114 MPa
<br>@Temperature 100 °C
16500 psi
<br>@Temperature 212 °F
4; ISO 527-2
186 MPa
<br>@Temperature 23.0 °C
27000 psi
<br>@Temperature 73.4 °F
4; ISO 527-2
Elongation at Break 1.7 %
1.7 %
ASTM D638
1.6 %
<br>@Temperature 23.0 °C
1.6 %
<br>@Temperature 73.4 °F
ISO 527-2
2.4 %
<br>@Temperature 100 °C
2.4 %
<br>@Temperature 212 °F
ISO 527-2
4.9 %
<br>@Temperature 175 °C
4.9 %
<br>@Temperature 347 °F
ISO 527-2
5.1 %
<br>@Temperature 150 °C
5.1 %
<br>@Temperature 302 °F
ISO 527-2
Tensile Modulus 13.7 GPa
1990 ksi
ASTM D638
5.10 GPa
<br>@Temperature 175 °C
740 ksi
<br>@Temperature 347 °F
4; ISO 527-2
5.90 GPa
<br>@Temperature 150 °C
856 ksi
<br>@Temperature 302 °F
4; ISO 527-2
9.20 GPa
<br>@Temperature 100 °C
1330 ksi
<br>@Temperature 212 °F
4; ISO 527-2
14.5 GPa
<br>@Temperature 23.0 °C
2100 ksi
<br>@Temperature 73.4 °F
4; ISO 527-2
Flexural Strength 229 MPa
33200 psi
ASTM D790
88.0 MPa
<br>@Temperature 175 °C
12800 psi
<br>@Temperature 347 °F
4; ISO 178
101 MPa
<br>@Temperature 150 °C
14600 psi
<br>@Temperature 302 °F
4; ISO 178
161 MPa
<br>@Temperature 100 °C
23400 psi
<br>@Temperature 212 °F
4; ISO 178
259 MPa
<br>@Temperature 23.0 °C
37600 psi
<br>@Temperature 73.4 °F
4; ISO 178
Flexural Modulus 13.3 GPa
1930 ksi
ASTM D790
4.60 GPa
<br>@Temperature 175 °C
667 ksi
<br>@Temperature 347 °F
ISO 178
5.00 GPa
<br>@Temperature 150 °C
725 ksi
<br>@Temperature 302 °F
ISO 178
8.10 GPa
<br>@Temperature 100 °C
1170 ksi
<br>@Temperature 212 °F
ISO 178
12.6 GPa
<br>@Temperature 23.0 °C
1830 ksi
<br>@Temperature 73.4 °F
ISO 178
Shear Strength 62.1 MPa
9010 psi
ASTM D732
Izod Impact, Notched 0.800 J/cm
1.50 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 8.00 kJ/m²
3.81 ft-lb/in²
Type 1, Notch A; ISO 180
Izod Impact, Unnotched (ISO) 44.0 kJ/m²
20.9 ft-lb/in²
Type 1; ISO 180
Charpy Impact Unnotched 4.70 J/cm²
22.4 ft-lb/in²
Type 1, Edgewise; ISO 179
Charpy Impact, Notched 1.40 J/cm²
6.66 ft-lb/in²
Type 1, Edgewise; ISO 179
Thermal Properties Metric English Comments
Melting Point 310 °C
590 °F
Peak; Dry; ASTM D3418
310 °C
590 °F
ISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 282 °C
540 °F
Unannealed; Flatwise; ISO 75-2/A
Processing Properties Metric English Comments
Rear Barrel Temperature 327 - 332 °C
621 - 630 °F
Middle Barrel Temperature 316 - 324 °C
601 - 615 °F
Front Barrel Temperature 316 - 324 °C
601 - 615 °F
Melt Temperature 321 - 338 °C
610 - 640 °F
Mold Temperature 65.6 - 93.3 °C
150 - 200 °F
Drying Temperature <= 120 °C
<br>@Time 14400 sec
<= 248 °F
<br>@Time 4.00 hour
Moisture Content 0.030 - 0.060 %
0.030 - 0.060 %
Suggested Max
Descriptive Properties Value Comments
Additive Flame Retardant
Availability Africa & Middle East
Asia Pacific
Europe
Latin America
North America
Color Black
Form Pellets
Part Marking Code >PA6T/66-GF33<
ISO 11469
Processing Technique Water-Heated Mold Injection Molding
Resin ID PA6T/66 GF33 FR(17)
ISO 1043
RoHS Compliance RoHS Compliant