Overview of materials for Polypropylene, Film Grade

Category Polymer , Film , Thermoplastic , Polypropylene (PP) , Polypropylene, Film Grade
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polypropylene, Film Grade.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene, Film Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.886 - 1.46 g/cc
0.0320 - 0.0527 lb/in³
Average value: 0.906 g/cc Grade Count:153
Water Vapor Transmission 0.0497 - 10.9 g/m²/day
0.00320 - 0.702 g/100 in²/day
Average value: 2.99 g/m²/day Grade Count:133
0.09312 - 18.624 g/m²/day

@Temperature 37.8 - 38.0 °C
0.005997 - 1.1994 g/100 in²/day

@Temperature 100 - 100 °F
Average value: 5.22 g/m²/day Grade Count:113
Oxygen Transmission Rate 0.0931 - 2100 cc/m²/day
0.00600 - 135 cc/100 in²/day
Average value: 375 cc/m²/day Grade Count:74
Thickness 12.0 - 96.5 microns
0.472 - 3.80 mil
Average value: 31.9 microns Grade Count:361
Linear Mold Shrinkage 0.0100 - 0.0400 cm/cm
0.0100 - 0.0400 in/in
Average value: 0.0346 cm/cm Grade Count:102
Linear Mold Shrinkage, Transverse 0.0100 - 0.0180 cm/cm
0.0100 - 0.0180 in/in
Average value: 0.0139 cm/cm Grade Count:101
Melt Flow 0.350 - 800 g/10 min
0.350 - 800 g/10 min
Average value: 9.85 g/10 min Grade Count:193
Ash 0.00100 - 0.00200 %
0.00100 - 0.00200 %
Average value: 0.00150 % Grade Count:7
Mechanical Properties Metric English Comments
Hardness, Rockwell R 65.0 - 113
65.0 - 113
Average value: 93.8 Grade Count:81
Hardness, Shore D 65.0 - 71.0
65.0 - 71.0
Average value: 68.5 Grade Count:4
Tensile Strength, Ultimate 18.8 - 152 MPa
2730 - 22000 psi
Average value: 42.9 MPa Grade Count:18
Film Tensile Strength at Yield, MD 3.00 - 31.5 MPa
435 - 4570 psi
Average value: 17.6 MPa Grade Count:15
Film Tensile Strength at Yield, TD 5.90 - 30.4 MPa
856 - 4410 psi
Average value: 16.5 MPa Grade Count:16
Tensile Strength, Yield 3.38 - 42.1 MPa
490 - 6110 psi
Average value: 32.7 MPa Grade Count:130
Film Elongation at Break, MD 80.0 - 850 %
80.0 - 850 %
Average value: 204 % Grade Count:299
Film Elongation at Break, TD 6.00 - 850 %
6.00 - 850 %
Average value: 86.4 % Grade Count:284
Elongation at Break 8.00 - 800 %
8.00 - 800 %
Average value: 444 % Grade Count:20
Elongation at Yield 7.00 - 20.0 %
7.00 - 20.0 %
Average value: 11.3 % Grade Count:106
Modulus of Elasticity 1.05 - 7.51 GPa
152 - 1090 ksi
Average value: 2.44 GPa Grade Count:112
Flexural Modulus 0.550 - 2.28 GPa
79.8 - 331 ksi
Average value: 1.38 GPa Grade Count:141
Secant Modulus 0.480 - 0.793 GPa
69.6 - 115 ksi
Average value: 0.625 GPa Grade Count:17
Secant Modulus, MD 0.400 - 2.90 GPa
58.0 - 420 ksi
Average value: 1.69 GPa Grade Count:25
Secant Modulus, TD 0.500 - 4.83 GPa
72.5 - 700 ksi
Average value: 2.65 GPa Grade Count:25
Izod Impact, Notched 0.196 - 5340 J/cm
0.367 - 10000 ft-lb/in
Average value: 0.436 J/cm Grade Count:107
0.180 - 0.267 J/cm

@Temperature -20.0 - 0.000 °C
0.337 - 0.500 ft-lb/in

@Temperature -4.00 - 32.0 °F
Average value: 0.215 J/cm Grade Count:4
Izod Impact, Unnotched 0.490 J/cm - NB
0.919 ft-lb/in - NB
Average value: 0.696 J/cm Grade Count:12
0.294199 - 0.294199 J/cm

@Temperature -10.0 - -10.0 °C
0.551156 - 0.551156 ft-lb/in

@Temperature 14.0 - 14.0 °F
Average value: 0.294 J/cm Grade Count:1
Izod Impact, Notched (ISO) 4.00 - 6.50 kJ/m²
1.90 - 3.09 ft-lb/in²
Average value: 5.15 kJ/m² Grade Count:13
Charpy Impact, Notched 0.500 - 55.0 J/cm²
2.38 - 262 ft-lb/in²
Average value: 6.07 J/cm² Grade Count:10
0.350 - 12.0 J/cm²

@Temperature -23.0 - 0.000 °C
1.67 - 57.1 ft-lb/in²

@Temperature -9.40 - 32.0 °F
Average value: 5.20 J/cm² Grade Count:3
Gardner Impact 1.40 - 36.2 J
1.03 - 26.7 ft-lb
Average value: 20.6 J Grade Count:6
28.4722 - 28.4722 J

@Temperature -30.0 - -29.0 °C
21.0000 - 21.0000 ft-lb

@Temperature -22.0 - -20.2 °F
Average value: 32.3 J Grade Count:2
Coefficient of Friction 0.170 - 0.900
0.170 - 0.900
Average value: 0.353 Grade Count:287
Elmendorf Tear Strength MD 12.0 - 64.0 g
12.0 - 64.0 g
Average value: 43.7 g Grade Count:3
Elmendorf Tear Strength TD 88.0 - 300 g
88.0 - 300 g
Average value: 176 g Grade Count:3
Elmendorf Tear Strength, MD 0.600 - 1.80 g/micron
15.2 - 45.7 g/mil
Average value: 1.40 g/micron Grade Count:5
Elmendorf Tear Strength, TD 2.00 - 9.00 g/micron
50.8 - 229 g/mil
Average value: 4.10 g/micron Grade Count:5
Dart Drop 0.780 - 9.40 g/micron
19.8 - 239 g/mil
Average value: 2.99 g/micron Grade Count:16
Dart Drop Test 20.0 - 350 g
0.0441 - 0.772 lb
Average value: 200 g Grade Count:8
Seal Strength 200 - 410 g/25 mm
200 - 410 g/in
Average value: 231 g/25 mm Grade Count:10
200 - 810 g/25 mm

@Temperature 80.0 - 140 °C
200 - 810 g/in

@Temperature 176 - 284 °F
Average value: 419 g/25 mm Grade Count:65
200 - 810 g/25 mm

@Pressure 0.00345 - 0.276 MPa
200 - 810 g/in

@Pressure 0.500 - 40.0 psi
Average value: 419 g/25 mm Grade Count:65
Film Tensile Strength at Break, MD 15.0 - 193 MPa
2180 - 28000 psi
Average value: 121 MPa Grade Count:382
Film Tensile Strength at Break, TD 8.00 - 310 MPa
1160 - 45000 psi
Average value: 231 MPa Grade Count:371
Tangent Modulus 869 - 1620 MPa
126000 - 235000 psi
Average value: 1120 MPa Grade Count:3
Heat Seal Strength 518 g/25 mm
1.14 lb/in
Average value: 518 g/25 mm Grade Count:48
Heat Seal Strength Initiation Temperature 105 - 130 °C
221 - 266 °F
Average value: 113 °C Grade Count:56
Thermal Properties Metric English Comments
Melting Point 119 - 170 °C
246 - 338 °F
Average value: 154 °C Grade Count:73
Deflection Temperature at 0.46 MPa (66 psi) 48.0 - 129 °C
118 - 264 °F
Average value: 95.3 °C Grade Count:109
Deflection Temperature at 1.8 MPa (264 psi) 50.0 - 104 °C
122 - 219 °F
Average value: 61.7 °C Grade Count:25
Electrical Properties Metric English Comments
Dielectric Constant 2.25
2.25
Average value: 2.25 Grade Count:7