| Category | Metal , Nonferrous Metal , Nickel Alloy , Superalloy |
| Manufacturer | Haynes International, Inc. |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Haynes 625 alloy, plate after 1000 hours at 760°C (1400°F).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.44 g/cc | 0.305 lb/in³ | at RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength, Ultimate | 985 MPa | 143000 psi | |
| Tensile Strength, Yield | 660 MPa <br>@Strain 0.200 % |
95700 psi <br>@Strain 0.200 % |
|
| Elongation at Break | 17 % | 17 % | in 50.8 mm |
| Modulus of Elasticity | 208 GPa | 30200 ksi | RT |
| 126 GPa <br>@Temperature 1000 °C |
18300 ksi <br>@Temperature 1830 °F |
||
| 142 GPa <br>@Temperature 900 °C |
20600 ksi <br>@Temperature 1650 °F |
||
| 153 GPa <br>@Temperature 800 °C |
22200 ksi <br>@Temperature 1470 °F |
||
| 163 GPa <br>@Temperature 700 °C |
23600 ksi <br>@Temperature 1290 °F |
||
| 171 GPa <br>@Temperature 600 °C |
24800 ksi <br>@Temperature 1110 °F |
||
| 179 GPa <br>@Temperature 500 °C |
26000 ksi <br>@Temperature 932 °F |
||
| 186 GPa <br>@Temperature 400 °C |
27000 ksi <br>@Temperature 752 °F |
||
| 192 GPa <br>@Temperature 300 °C |
27800 ksi <br>@Temperature 572 °F |
||
| 199 GPa <br>@Temperature 200 °C |
28900 ksi <br>@Temperature 392 °F |
||
| 201 GPa <br>@Temperature 100 °C |
29200 ksi <br>@Temperature 212 °F |
||
| Charpy Impact | 7.00 J | 5.16 ft-lb |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 12.8 µm/m-°C <br>@Temperature 25.0 - 100 °C |
7.11 µin/in-°F <br>@Temperature 77.0 - 212 °F |
|
| 13.1 µm/m-°C <br>@Temperature 25.0 - 200 °C |
7.28 µin/in-°F <br>@Temperature 77.0 - 392 °F |
||
| 13.4 µm/m-°C <br>@Temperature 25.0 - 300 °C |
7.44 µin/in-°F <br>@Temperature 77.0 - 572 °F |
||
| 13.8 µm/m-°C <br>@Temperature 25.0 - 400 °C |
7.67 µin/in-°F <br>@Temperature 77.0 - 752 °F |
||
| 14.2 µm/m-°C <br>@Temperature 25.0 - 500 °C |
7.89 µin/in-°F <br>@Temperature 77.0 - 932 °F |
||
| 14.8 µm/m-°C <br>@Temperature 25.0 - 600 °C |
8.22 µin/in-°F <br>@Temperature 77.0 - 1110 °F |
||
| 15.4 µm/m-°C <br>@Temperature 25.0 - 700 °C |
8.56 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
||
| 16.0 µm/m-°C <br>@Temperature 25.0 - 800 °C |
8.89 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 16.7 µm/m-°C <br>@Temperature 25.0 - 900 °C |
9.28 µin/in-°F <br>@Temperature 77.0 - 1650 °F |
||
| 17.4 µm/m-°C <br>@Temperature 25.0 - 1000 °C |
9.67 µin/in-°F <br>@Temperature 77.0 - 1830 °F |
||
| Specific Heat Capacity | 0.410 J/g-°C | 0.0980 BTU/lb-°F | RT |
| 0.428 J/g-°C <br>@Temperature 100 °C |
0.102 BTU/lb-°F <br>@Temperature 212 °F |
||
| 0.455 J/g-°C <br>@Temperature 200 °C |
0.109 BTU/lb-°F <br>@Temperature 392 °F |
||
| 0.477 J/g-°C <br>@Temperature 300 °C |
0.114 BTU/lb-°F <br>@Temperature 572 °F |
||
| 0.503 J/g-°C <br>@Temperature 400 °C |
0.120 BTU/lb-°F <br>@Temperature 752 °F |
||
| 0.527 J/g-°C <br>@Temperature 500 °C |
0.126 BTU/lb-°F <br>@Temperature 932 °F |
||
| 0.552 J/g-°C <br>@Temperature 600 °C |
0.132 BTU/lb-°F <br>@Temperature 1110 °F |
||
| 0.576 J/g-°C <br>@Temperature 700 °C |
0.138 BTU/lb-°F <br>@Temperature 1290 °F |
||
| 0.600 J/g-°C <br>@Temperature 800 °C |
0.143 BTU/lb-°F <br>@Temperature 1470 °F |
||
| 0.625 J/g-°C <br>@Temperature 900 °C |
0.149 BTU/lb-°F <br>@Temperature 1650 °F |
||
| 0.648 J/g-°C <br>@Temperature 1000 °C |
0.155 BTU/lb-°F <br>@Temperature 1830 °F |
||
| Thermal Conductivity | 9.80 W/m-K | 68.0 BTU-in/hr-ft²-°F | RT |
| 10.9 W/m-K <br>@Temperature 100 °C |
75.6 BTU-in/hr-ft²-°F <br>@Temperature 212 °F |
||
| 12.5 W/m-K <br>@Temperature 200 °C |
86.8 BTU-in/hr-ft²-°F <br>@Temperature 392 °F |
||
| 13.9 W/m-K <br>@Temperature 300 °C |
96.5 BTU-in/hr-ft²-°F <br>@Temperature 572 °F |
||
| 15.3 W/m-K <br>@Temperature 400 °C |
106 BTU-in/hr-ft²-°F <br>@Temperature 752 °F |
||
| 16.9 W/m-K <br>@Temperature 500 °C |
117 BTU-in/hr-ft²-°F <br>@Temperature 932 °F |
||
| 18.3 W/m-K <br>@Temperature 600 °C |
127 BTU-in/hr-ft²-°F <br>@Temperature 1110 °F |
||
| 19.8 W/m-K <br>@Temperature 700 °C |
137 BTU-in/hr-ft²-°F <br>@Temperature 1290 °F |
||
| 21.5 W/m-K <br>@Temperature 800 °C |
149 BTU-in/hr-ft²-°F <br>@Temperature 1470 °F |
||
| 23.4 W/m-K <br>@Temperature 900 °C |
162 BTU-in/hr-ft²-°F <br>@Temperature 1650 °F |
||
| 25.6 W/m-K <br>@Temperature 1000 °C |
178 BTU-in/hr-ft²-°F <br>@Temperature 1830 °F |
||
| Melting Point | 1290 - 1350 °C | 2350 - 2460 °F | |
| Solidus | 1290 °C | 2350 °F | |
| Liquidus | 1350 °C | 2460 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Aluminum, Al | <= 0.40 % | <= 0.40 % | |
| Carbon, C | <= 0.10 % | <= 0.10 % | |
| Chromium, Cr | 21 % | 21 % | |
| Cobalt, Co | <= 1.0 % | <= 1.0 % | |
| Iron, Fe | <= 5.0 % | <= 5.0 % | |
| Manganese, Mn | <= 0.50 % | <= 0.50 % | |
| Molybdenum, Mo | 9.0 % | 9.0 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.000129 ohm-cm | 0.000129 ohm-cm | RT |
| 0.000132 ohm-cm <br>@Temperature 100 °C |
0.000132 ohm-cm <br>@Temperature 212 °F |
||
| 0.000134 ohm-cm <br>@Temperature 200 °C |
0.000134 ohm-cm <br>@Temperature 392 °F |
||
| 0.000135 ohm-cm <br>@Temperature 300 °C |
0.000135 ohm-cm <br>@Temperature 572 °F |
||
| 0.000135 ohm-cm <br>@Temperature 1000 °C |
0.000135 ohm-cm <br>@Temperature 1830 °F |
||
| 0.000136 ohm-cm <br>@Temperature 900 °C |
0.000136 ohm-cm <br>@Temperature 1650 °F |
||
| 0.000136 ohm-cm <br>@Temperature 400 °C |
0.000136 ohm-cm <br>@Temperature 752 °F |
||
| 0.000137 ohm-cm <br>@Temperature 500 °C |
0.000137 ohm-cm <br>@Temperature 932 °F |
||
| 0.000137 ohm-cm <br>@Temperature 800 °C |
0.000137 ohm-cm <br>@Temperature 1470 °F |
||
| 0.000138 ohm-cm <br>@Temperature 600 °C |
0.000138 ohm-cm <br>@Temperature 1110 °F |
||
| 0.000138 ohm-cm <br>@Temperature 700 °C |
0.000138 ohm-cm <br>@Temperature 1290 °F |