| Category | Metal , Nonferrous Metal , Nickel Alloy , Superalloy |
| Manufacturer | Haynes International, Inc. |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Haynes 242® alloy, cold reduced sheet, annealed, 40% cold work, aged.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 9.05 g/cc | 0.327 lb/in³ | at RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 257 | 257 | Converted from Vickers hardness |
| Hardness, Knoop | 286 | 286 | Converted from Vickers hardness |
| Hardness, Rockwell C | 19 | 19 | Converted from Vickers hardness |
| Hardness, Vickers | 78.0 <br>@Temperature 870 °C |
78.0 <br>@Temperature 1600 °F |
|
| 140 <br>@Temperature 760 °C |
140 <br>@Temperature 1400 °F |
||
| 218 <br>@Temperature 650 °C |
218 <br>@Temperature 1200 °F |
||
| 263 <br>@Temperature 540 °C |
263 <br>@Temperature 1000 °F |
||
| 271 <br>@Temperature 425 °C |
271 <br>@Temperature 797 °F |
||
| Tensile Strength, Ultimate | 1685 MPa | 244400 psi | |
| 1075 MPa <br>@Temperature 760 °C |
155900 psi <br>@Temperature 1400 °F |
||
| 1265 MPa <br>@Temperature 705 °C |
183500 psi <br>@Temperature 1300 °F |
||
| 1370 MPa <br>@Temperature 650 °C |
199000 psi <br>@Temperature 1200 °F |
||
| 1390 MPa <br>@Temperature 595 °C |
202000 psi <br>@Temperature 1100 °F |
||
| Tensile Strength, Yield | 1515 MPa <br>@Strain 0.200 % |
219700 psi <br>@Strain 0.200 % |
|
| 650 MPa <br>@Strain 0.200 %,<br> Temperature 760 °C |
94300 psi <br>@Strain 0.200 %,<br> Temperature 1400 °F |
||
| 925 MPa <br>@Strain 0.200 %,<br> Temperature 705 °C |
134000 psi <br>@Strain 0.200 %,<br> Temperature 1300 °F |
||
| 1005 MPa <br>@Strain 0.200 %,<br> Temperature 650 °C |
145800 psi <br>@Strain 0.200 %,<br> Temperature 1200 °F |
||
| 1320 MPa <br>@Strain 0.200 %,<br> Temperature 595 °C |
191000 psi <br>@Strain 0.200 %,<br> Temperature 1100 °F |
||
| Elongation at Break | 11 % | 11 % | in 50 mm |
| 8.0 % <br>@Temperature 650 °C |
8.0 % <br>@Temperature 1200 °F |
in 50 mm | |
| 11 % <br>@Temperature 705 °C |
11 % <br>@Temperature 1300 °F |
in 50 mm | |
| 11 % <br>@Temperature 595 °C |
11 % <br>@Temperature 1100 °F |
in 50 mm | |
| 32 % <br>@Temperature 760 °C |
32 % <br>@Temperature 1400 °F |
in 50 mm | |
| Modulus of Elasticity | 229 GPa | 33200 ksi | RT |
| 152 GPa <br>@Temperature 1000 °C |
22000 ksi <br>@Temperature 1830 °F |
||
| 163 GPa <br>@Temperature 900 °C |
23600 ksi <br>@Temperature 1650 °F |
||
| 172 GPa <br>@Temperature 800 °C |
24900 ksi <br>@Temperature 1470 °F |
||
| 185 GPa <br>@Temperature 700 °C |
26800 ksi <br>@Temperature 1290 °F |
||
| 193 GPa <br>@Temperature 600 °C |
28000 ksi <br>@Temperature 1110 °F |
||
| 199 GPa <br>@Temperature 500 °C |
28900 ksi <br>@Temperature 932 °F |
||
| 206 GPa <br>@Temperature 400 °C |
29900 ksi <br>@Temperature 752 °F |
||
| 213 GPa <br>@Temperature 300 °C |
30900 ksi <br>@Temperature 572 °F |
||
| 219 GPa <br>@Temperature 200 °C |
31800 ksi <br>@Temperature 392 °F |
||
| 225 GPa <br>@Temperature 100 °C |
32600 ksi <br>@Temperature 212 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 10.8 µm/m-°C <br>@Temperature 25.0 - 100 °C |
6.00 µin/in-°F <br>@Temperature 77.0 - 212 °F |
|
| 11.3 µm/m-°C <br>@Temperature 25.0 - 200 °C |
6.28 µin/in-°F <br>@Temperature 77.0 - 392 °F |
||
| 11.6 µm/m-°C <br>@Temperature 25.0 - 300 °C |
6.44 µin/in-°F <br>@Temperature 77.0 - 572 °F |
||
| 11.9 µm/m-°C <br>@Temperature 25.0 - 400 °C |
6.61 µin/in-°F <br>@Temperature 77.0 - 752 °F |
||
| 12.2 µm/m-°C <br>@Temperature 25.0 - 500 °C |
6.78 µin/in-°F <br>@Temperature 77.0 - 932 °F |
||
| 12.3 µm/m-°C <br>@Temperature 25.0 - 600 °C |
6.83 µin/in-°F <br>@Temperature 77.0 - 1110 °F |
||
| 12.4 µm/m-°C <br>@Temperature 25.0 - 650 °C |
6.89 µin/in-°F <br>@Temperature 77.0 - 1200 °F |
||
| 13.0 µm/m-°C <br>@Temperature 25.0 - 700 °C |
7.22 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
||
| 13.7 µm/m-°C <br>@Temperature 25.0 - 750 °C |
7.61 µin/in-°F <br>@Temperature 77.0 - 1380 °F |
||
| 14.0 µm/m-°C <br>@Temperature 25.0 - 800 °C |
7.78 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 14.5 µm/m-°C <br>@Temperature 25.0 - 900 °C |
8.06 µin/in-°F <br>@Temperature 77.0 - 1650 °F |
||
| 15.0 µm/m-°C <br>@Temperature 25.0 - 1000 °C |
8.33 µin/in-°F <br>@Temperature 77.0 - 1830 °F |
||
| Specific Heat Capacity | 0.386 J/g-°C | 0.0923 BTU/lb-°F | RT |
| 0.405 J/g-°C <br>@Temperature 100 °C |
0.0968 BTU/lb-°F <br>@Temperature 212 °F |
||
| 0.419 J/g-°C <br>@Temperature 200 °C |
0.100 BTU/lb-°F <br>@Temperature 392 °F |
||
| 0.431 J/g-°C <br>@Temperature 300 °C |
0.103 BTU/lb-°F <br>@Temperature 572 °F |
||
| 0.439 J/g-°C <br>@Temperature 400 °C |
0.105 BTU/lb-°F <br>@Temperature 752 °F |
||
| 0.451 J/g-°C <br>@Temperature 500 °C |
0.108 BTU/lb-°F <br>@Temperature 932 °F |
||
| 0.470 J/g-°C <br>@Temperature 600 °C |
0.112 BTU/lb-°F <br>@Temperature 1110 °F |
||
| 0.595 J/g-°C <br>@Temperature 700 °C |
0.142 BTU/lb-°F <br>@Temperature 1290 °F |
||
| 0.605 J/g-°C <br>@Temperature 800 °C |
0.145 BTU/lb-°F <br>@Temperature 1470 °F |
||
| 0.610 J/g-°C <br>@Temperature 900 °C |
0.146 BTU/lb-°F <br>@Temperature 1650 °F |
||
| 0.627 J/g-°C <br>@Temperature 1000 °C |
0.150 BTU/lb-°F <br>@Temperature 1830 °F |
||
| Thermal Conductivity | 11.3 W/m-K | 78.4 BTU-in/hr-ft²-°F | RT |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.000122 ohm-cm | 0.000122 ohm-cm | RT |
| 0.0001234 ohm-cm <br>@Temperature 100 °C |
0.0001234 ohm-cm <br>@Temperature 212 °F |
||
| 0.0001251 ohm-cm <br>@Temperature 200 °C |
0.0001251 ohm-cm <br>@Temperature 392 °F |
||
| 0.0001267 ohm-cm <br>@Temperature 300 °C |
0.0001267 ohm-cm <br>@Temperature 572 °F |
||
| 0.0001276 ohm-cm <br>@Temperature 1000 °C |
0.0001276 ohm-cm <br>@Temperature 1830 °F |
||
| 0.000128 ohm-cm <br>@Temperature 400 °C |
0.000128 ohm-cm <br>@Temperature 752 °F |
||
| 0.0001295 ohm-cm <br>@Temperature 500 °C |
0.0001295 ohm-cm <br>@Temperature 932 °F |
||
| 0.0001298 ohm-cm <br>@Temperature 900 °C |
0.0001298 ohm-cm <br>@Temperature 1650 °F |
||
| 0.0001306 ohm-cm <br>@Temperature 600 °C |
0.0001306 ohm-cm <br>@Temperature 1110 °F |
||
| 0.000132 ohm-cm <br>@Temperature 700 °C |
0.000132 ohm-cm <br>@Temperature 1290 °F |
||
| 0.0001324 ohm-cm <br>@Temperature 800 °C |
0.0001324 ohm-cm <br>@Temperature 1470 °F |