| Category | Metal , Nonferrous Metal , Nickel Alloy , Superalloy |
| Manufacturer | Haynes International, Inc. |
| Trade Name | |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Haynes 230® alloy, GMAW deposit weld metal.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.97 g/cc | 0.324 lb/in³ | at RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength, Ultimate | 785 MPa | 114000 psi | |
| 310 MPa <br>@Temperature 871 °C |
45000 psi <br>@Temperature 1600 °F |
||
| 610 MPa <br>@Temperature 538 °C |
88500 psi <br>@Temperature 1000 °F |
||
| Tensile Strength, Yield | 490 MPa <br>@Strain 0.200 % |
71100 psi <br>@Strain 0.200 % |
|
| 275 MPa <br>@Strain 0.200 %,<br> Temperature 871 °C |
39900 psi <br>@Strain 0.200 %,<br> Temperature 1600 °F |
||
| 435 MPa <br>@Strain 0.200 %,<br> Temperature 538 °C |
63100 psi <br>@Strain 0.200 %,<br> Temperature 1000 °F |
||
| Elongation at Break | 48.2 % | 48.2 % | in 50.8 mm |
| 34.8 % <br>@Temperature 538 °C |
34.8 % <br>@Temperature 1000 °F |
in 50.8 mm | |
| 45.4 % <br>@Temperature 871 °C |
45.4 % <br>@Temperature 1600 °F |
in 50.8 mm | |
| Modulus of Elasticity | 211 GPa | 30600 ksi | RT |
| 150 GPa <br>@Temperature 1000 °C |
21800 ksi <br>@Temperature 1830 °F |
||
| 157 GPa <br>@Temperature 900 °C |
22800 ksi <br>@Temperature 1650 °F |
||
| 164 GPa <br>@Temperature 800 °C |
23800 ksi <br>@Temperature 1470 °F |
||
| 171 GPa <br>@Temperature 700 °C |
24800 ksi <br>@Temperature 1290 °F |
||
| 177 GPa <br>@Temperature 600 °C |
25700 ksi <br>@Temperature 1110 °F |
||
| 184 GPa <br>@Temperature 500 °C |
26700 ksi <br>@Temperature 932 °F |
||
| 190 GPa <br>@Temperature 400 °C |
27600 ksi <br>@Temperature 752 °F |
||
| 196 GPa <br>@Temperature 300 °C |
28400 ksi <br>@Temperature 572 °F |
||
| 202 GPa <br>@Temperature 200 °C |
29300 ksi <br>@Temperature 392 °F |
||
| 207 GPa <br>@Temperature 100 °C |
30000 ksi <br>@Temperature 212 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 12.7 µm/m-°C <br>@Temperature 25.0 - 100 °C |
7.06 µin/in-°F <br>@Temperature 77.0 - 212 °F |
|
| 13.0 µm/m-°C <br>@Temperature 25.0 - 200 °C |
7.22 µin/in-°F <br>@Temperature 77.0 - 392 °F |
||
| 13.3 µm/m-°C <br>@Temperature 25.0 - 300 °C |
7.39 µin/in-°F <br>@Temperature 77.0 - 572 °F |
||
| 13.7 µm/m-°C <br>@Temperature 25.0 - 400 °C |
7.61 µin/in-°F <br>@Temperature 77.0 - 752 °F |
||
| 14.0 µm/m-°C <br>@Temperature 25.0 - 500 °C |
7.78 µin/in-°F <br>@Temperature 77.0 - 932 °F |
||
| 14.4 µm/m-°C <br>@Temperature 25.0 - 600 °C |
8.00 µin/in-°F <br>@Temperature 77.0 - 1110 °F |
||
| 14.8 µm/m-°C <br>@Temperature 25.0 - 700 °C |
8.22 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
||
| 15.2 µm/m-°C <br>@Temperature 25.0 - 800 °C |
8.44 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 15.7 µm/m-°C <br>@Temperature 25.0 - 900 °C |
8.72 µin/in-°F <br>@Temperature 77.0 - 1650 °F |
||
| 16.1 µm/m-°C <br>@Temperature 25.0 - 1000 °C |
8.94 µin/in-°F <br>@Temperature 77.0 - 1830 °F |
||
| Specific Heat Capacity | 0.397 J/g-°C | 0.0949 BTU/lb-°F | RT |
| 0.419 J/g-°C <br>@Temperature 100 °C |
0.100 BTU/lb-°F <br>@Temperature 212 °F |
||
| 0.435 J/g-°C <br>@Temperature 200 °C |
0.104 BTU/lb-°F <br>@Temperature 392 °F |
||
| 0.448 J/g-°C <br>@Temperature 300 °C |
0.107 BTU/lb-°F <br>@Temperature 572 °F |
||
| 0.465 J/g-°C <br>@Temperature 400 °C |
0.111 BTU/lb-°F <br>@Temperature 752 °F |
||
| 0.473 J/g-°C <br>@Temperature 500 °C |
0.113 BTU/lb-°F <br>@Temperature 932 °F |
||
| 0.486 J/g-°C <br>@Temperature 600 °C |
0.116 BTU/lb-°F <br>@Temperature 1110 °F |
||
| 0.574 J/g-°C <br>@Temperature 700 °C |
0.137 BTU/lb-°F <br>@Temperature 1290 °F |
||
| 0.595 J/g-°C <br>@Temperature 800 °C |
0.142 BTU/lb-°F <br>@Temperature 1470 °F |
||
| 0.609 J/g-°C <br>@Temperature 900 °C |
0.146 BTU/lb-°F <br>@Temperature 1650 °F |
||
| 0.617 J/g-°C <br>@Temperature 1000 °C |
0.147 BTU/lb-°F <br>@Temperature 1830 °F |
||
| Thermal Conductivity | 8.90 W/m-K | 61.8 BTU-in/hr-ft²-°F | RT |
| 10.4 W/m-K <br>@Temperature 100 °C |
72.2 BTU-in/hr-ft²-°F <br>@Temperature 212 °F |
||
| 12.4 W/m-K <br>@Temperature 200 °C |
86.1 BTU-in/hr-ft²-°F <br>@Temperature 392 °F |
||
| 14.4 W/m-K <br>@Temperature 300 °C |
99.9 BTU-in/hr-ft²-°F <br>@Temperature 572 °F |
||
| 16.4 W/m-K <br>@Temperature 400 °C |
114 BTU-in/hr-ft²-°F <br>@Temperature 752 °F |
||
| 18.4 W/m-K <br>@Temperature 500 °C |
128 BTU-in/hr-ft²-°F <br>@Temperature 932 °F |
||
| 20.4 W/m-K <br>@Temperature 600 °C |
142 BTU-in/hr-ft²-°F <br>@Temperature 1110 °F |
||
| 22.4 W/m-K <br>@Temperature 700 °C |
155 BTU-in/hr-ft²-°F <br>@Temperature 1290 °F |
||
| 24.4 W/m-K <br>@Temperature 800 °C |
169 BTU-in/hr-ft²-°F <br>@Temperature 1470 °F |
||
| 26.4 W/m-K <br>@Temperature 900 °C |
183 BTU-in/hr-ft²-°F <br>@Temperature 1650 °F |
||
| 28.4 W/m-K <br>@Temperature 1000 °C |
197 BTU-in/hr-ft²-°F <br>@Temperature 1830 °F |
||
| Melting Point | 1301 - 1371 °C | 2374 - 2500 °F | |
| Solidus | 1301 °C | 2374 °F |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.000125 ohm-cm | 0.000125 ohm-cm | RT |
| 0.000125 ohm-cm <br>@Temperature 1000 °C |
0.000125 ohm-cm <br>@Temperature 1830 °F |
||
| 0.0001258 ohm-cm <br>@Temperature 100 °C |
0.0001258 ohm-cm <br>@Temperature 212 °F |
||
| 0.0001265 ohm-cm <br>@Temperature 200 °C |
0.0001265 ohm-cm <br>@Temperature 392 °F |
||
| 0.0001271 ohm-cm <br>@Temperature 900 °C |
0.0001271 ohm-cm <br>@Temperature 1650 °F |
||
| 0.0001273 ohm-cm <br>@Temperature 300 °C |
0.0001273 ohm-cm <br>@Temperature 572 °F |
||
| 0.0001284 ohm-cm <br>@Temperature 400 °C |
0.0001284 ohm-cm <br>@Temperature 752 °F |
||
| 0.0001291 ohm-cm <br>@Temperature 800 °C |
0.0001291 ohm-cm <br>@Temperature 1470 °F |
||
| 0.0001302 ohm-cm <br>@Temperature 500 °C |
0.0001302 ohm-cm <br>@Temperature 932 °F |
||
| 0.0001307 ohm-cm <br>@Temperature 700 °C |
0.0001307 ohm-cm <br>@Temperature 1290 °F |
||
| 0.0001312 ohm-cm <br>@Temperature 600 °C |
0.0001312 ohm-cm <br>@Temperature 1110 °F |