| Category | Metal , Nonferrous Metal , Nickel Alloy , Superalloy | 
| Manufacturer | Haynes International, Inc. | 
| Trade Name | |
| Port | Ningbo port,China | 
| Trade Terms | FOB, CFR, CIF | 
| Payment Terms | L/C, T/T, Western Union | 
| Download PDF | Haynes 214® alloy, 20% cold reduction, 980°C (1800°F) for 5 minutes.pdf  | 
| Price | EMAIL US sales@lookpolymers.com | 
| Physical Properties | Metric | English | Comments | 
|---|---|---|---|
| Density | 8.05 g/cc | 0.291 lb/in³ | at RT | 
| Mechanical Properties | Metric | English | Comments | 
|---|---|---|---|
| Hardness, Brinell | 261 | 261 | Converted from Rockwell C hardness. | 
| Hardness, Knoop | 283 | 283 | Converted from Rockwell C hardness. | 
| Hardness, Rockwell C | 24.9 | 24.9 | |
| Hardness, Vickers | 268 | 268 | Converted from Rockwell C hardness. | 
| Tensile Strength, Ultimate | 1035 MPa | 150100 psi | |
| Tensile Strength, Yield | 620           MPa @Strain 0.200 % | 89900           psi @Strain 0.200 % | |
| Elongation at Break | 33.7 % | 33.7 % | in 50.8 mm | 
| Modulus of Elasticity | 218 GPa | 31600 ksi | RT | 
| 137           GPa @Temperature 1000 °C | 19900           ksi @Temperature 1830 °F | ||
| 151           GPa @Temperature 900 °C | 21900           ksi @Temperature 1650 °F | ||
| 162           GPa @Temperature 800 °C | 23500           ksi @Temperature 1470 °F | ||
| 170           GPa @Temperature 700 °C | 24700           ksi @Temperature 1290 °F | ||
| 177           GPa @Temperature 600 °C | 25700           ksi @Temperature 1110 °F | ||
| 184           GPa @Temperature 500 °C | 26700           ksi @Temperature 932 °F | ||
| 190           GPa @Temperature 400 °C | 27600           ksi @Temperature 752 °F | ||
| 199           GPa @Temperature 300 °C | 28900           ksi @Temperature 572 °F | ||
| 204           GPa @Temperature 200 °C | 29600           ksi @Temperature 392 °F | ||
| 210           GPa @Temperature 100 °C | 30500           ksi @Temperature 212 °F | 
| Thermal Properties | Metric | English | Comments | 
|---|---|---|---|
| CTE, linear | 13.3           µm/m-°C @Temperature 25.0 - 200 °C | 7.39           µin/in-°F @Temperature 77.0 - 392 °F | |
| 13.6           µm/m-°C @Temperature 25.0 - 300 °C | 7.56           µin/in-°F @Temperature 77.0 - 572 °F | ||
| 14.1           µm/m-°C @Temperature 25.0 - 400 °C | 7.83           µin/in-°F @Temperature 77.0 - 752 °F | ||
| 14.6           µm/m-°C @Temperature 25.0 - 500 °C | 8.11           µin/in-°F @Temperature 77.0 - 932 °F | ||
| 15.2           µm/m-°C @Temperature 25.0 - 600 °C | 8.44           µin/in-°F @Temperature 77.0 - 1110 °F | ||
| 15.8           µm/m-°C @Temperature 25.0 - 700 °C | 8.78           µin/in-°F @Temperature 77.0 - 1290 °F | ||
| 16.6           µm/m-°C @Temperature 25.0 - 800 °C | 9.22           µin/in-°F @Temperature 77.0 - 1470 °F | ||
| 17.6           µm/m-°C @Temperature 25.0 - 900 °C | 9.78           µin/in-°F @Temperature 77.0 - 1650 °F | ||
| 18.6           µm/m-°C @Temperature 25.0 - 1000 °C | 10.3           µin/in-°F @Temperature 77.0 - 1830 °F | ||
| Specific Heat Capacity | 0.452 J/g-°C | 0.108 BTU/lb-°F | RT | 
| 0.470           J/g-°C @Temperature 100 °C | 0.112           BTU/lb-°F @Temperature 212 °F | ||
| 0.493           J/g-°C @Temperature 200 °C | 0.118           BTU/lb-°F @Temperature 392 °F | ||
| 0.515           J/g-°C @Temperature 300 °C | 0.123           BTU/lb-°F @Temperature 572 °F | ||
| 0.538           J/g-°C @Temperature 400 °C | 0.129           BTU/lb-°F @Temperature 752 °F | ||
| 0.561           J/g-°C @Temperature 500 °C | 0.134           BTU/lb-°F @Temperature 932 °F | ||
| 0.611           J/g-°C @Temperature 600 °C | 0.146           BTU/lb-°F @Temperature 1110 °F | ||
| 0.668           J/g-°C @Temperature 700 °C | 0.160           BTU/lb-°F @Temperature 1290 °F | ||
| 0.705           J/g-°C @Temperature 800 °C | 0.168           BTU/lb-°F @Temperature 1470 °F | ||
| 0.728           J/g-°C @Temperature 900 °C | 0.174           BTU/lb-°F @Temperature 1650 °F | ||
| 0.742           J/g-°C @Temperature 1000 °C | 0.177           BTU/lb-°F @Temperature 1830 °F | ||
| 0.749           J/g-°C @Temperature 1100 °C | 0.179           BTU/lb-°F @Temperature 2010 °F | ||
| 0.753           J/g-°C @Temperature 1200 °C | 0.180           BTU/lb-°F @Temperature 2190 °F | ||
| Thermal Conductivity | 12.0 W/m-K | 83.3 BTU-in/hr-ft²-°F | RT | 
| 12.8           W/m-K @Temperature 100 °C | 88.8           BTU-in/hr-ft²-°F @Temperature 212 °F | ||
| 14.2           W/m-K @Temperature 200 °C | 98.5           BTU-in/hr-ft²-°F @Temperature 392 °F | ||
| 15.9           W/m-K @Temperature 300 °C | 110           BTU-in/hr-ft²-°F @Temperature 572 °F | ||
| 18.4           W/m-K @Temperature 400 °C | 128           BTU-in/hr-ft²-°F @Temperature 752 °F | ||
| 21.1           W/m-K @Temperature 500 °C | 146           BTU-in/hr-ft²-°F @Temperature 932 °F | ||
| 23.9           W/m-K @Temperature 600 °C | 166           BTU-in/hr-ft²-°F @Temperature 1110 °F | ||
| 26.9           W/m-K @Temperature 700 °C | 187           BTU-in/hr-ft²-°F @Temperature 1290 °F | ||
| 29.7           W/m-K @Temperature 800 °C | 206           BTU-in/hr-ft²-°F @Temperature 1470 °F | ||
| 31.4           W/m-K @Temperature 900 °C | 218           BTU-in/hr-ft²-°F @Temperature 1650 °F | 
| Electrical Properties | Metric | English | Comments | 
|---|---|---|---|
| Electrical Resistivity | 0.0001359 ohm-cm | 0.0001359 ohm-cm | RT | 
| 0.0001209           ohm-cm @Temperature 1050 °C | 0.0001209           ohm-cm @Temperature 1920 °F | ||
| 0.000121           ohm-cm @Temperature 1100 °C | 0.000121           ohm-cm @Temperature 2010 °F | ||
| 0.0001216           ohm-cm @Temperature 1000 °C | 0.0001216           ohm-cm @Temperature 1830 °F | ||
| 0.0001219           ohm-cm @Temperature 1150 °C | 0.0001219           ohm-cm @Temperature 2100 °F | ||
| 0.0001229           ohm-cm @Temperature 1200 °C | 0.0001229           ohm-cm @Temperature 2190 °F | ||
| 0.0001249           ohm-cm @Temperature 900 °C | 0.0001249           ohm-cm @Temperature 1650 °F | ||
| 0.0001292           ohm-cm @Temperature 800 °C | 0.0001292           ohm-cm @Temperature 1470 °F | ||
| 0.0001337           ohm-cm @Temperature 700 °C | 0.0001337           ohm-cm @Temperature 1290 °F | ||
| 0.0001368           ohm-cm @Temperature 600 °C | 0.0001368           ohm-cm @Temperature 1110 °F | ||
| 0.0001369           ohm-cm @Temperature 100 °C | 0.0001369           ohm-cm @Temperature 212 °F | ||
| 0.0001369           ohm-cm @Temperature 200 °C | 0.0001369           ohm-cm @Temperature 392 °F | ||
| 0.0001369           ohm-cm @Temperature 300 °C | 0.0001369           ohm-cm @Temperature 572 °F | ||
| 0.0001369           ohm-cm @Temperature 300 °C | 0.0001369           ohm-cm @Temperature 572 °F | ||
| 0.0001377           ohm-cm @Temperature 400 °C | 0.0001377           ohm-cm @Temperature 752 °F | ||
| 0.0001379           ohm-cm @Temperature 500 °C | 0.0001379           ohm-cm @Temperature 932 °F |