Eagle Brass 706 Copper Nickel 10%, Annealed

Category Metal , Nonferrous Metal , Copper Alloy
Manufacturer Eagle Brass Company
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Eagle Brass 706 Copper Nickel 10%, Annealed.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
706 exhibits excellent corrosion resistance, especially in marine applications. It has a relatively high strength and has resistance at elevated temperatures. The cost is relatively high compared to copper-aluminum and other alloys with similar mechanical properties.Typical uses include brake lines, screw lamp bases, boat hulls, pipe fittings, heat exchanger tubes, and flanges.Information provided by Eagle Brass Company
Physical Properties Metric English Comments
Density 8.94 g/cc
0.323 lb/in³
Annealed
Mechanical Properties Metric English Comments
Hardness, Rockwell 30T 15 - 45
15 - 45
Thickness > 0.020 Inch
Tensile Strength, Ultimate 296 - 345 MPa
43000 - 50000 psi
Tensile Strength, Yield 89.6 - 172 MPa
13000 - 25000 psi
0.2% offset
Elongation at Break 33 - 37 %
33 - 37 %
in 2 in.
Tensile Modulus 124 GPa
18000 ksi
Thermal Properties Metric English Comments
CTE, linear 17.1 µm/m-°C

@Temperature 20.0 - 300 °C
9.50 µin/in-°F

@Temperature 68.0 - 572 °F
Thermal Conductivity 45.0 W/m-K
312 BTU-in/hr-ft²-°F
Component Elements Properties Metric English Comments
Copper, Cu 88.6 %
88.6 %
Iron, Fe 1.4 %
1.4 %
Nickel, Ni 10 %
10 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.0000198 ohm-cm
0.0000198 ohm-cm
Annealed